Nanometer needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies as well as preparation method and application of nanometer needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material

By growing nano-acid nickel-cobalt sulfide on the surface of the carbon cloth, introducing sulfur vacancy defects and adjusting the structure, the problems of poor mechanical properties and impedance mismatch of traditional electromagnetic wave absorbers are solved, and efficient electromagnetic wave absorption performance is achieved, especially in Excellent performance and wide band applications in the 2–18GHz frequency range.

CN119020991APending Publication Date: 2024-11-26GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115200.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional electromagnetic wave absorbers have poor mechanical properties, and the high conductivity and impedance mismatch of carbon cloth lead to electromagnetic wave reflection, reducing absorption performance. How to grow transition metal sulfides on the surface of carbon cloth and introduce vacancy defects to improve electromagnetic wave absorption performance.

Method used

The growth of nanoneedle-shaped nickel-cobalt sulfide on the surface of the carbon cloth through hydrothermal reaction and high-temperature annealing process, introducing a large number of sulfur vacancy defects, adjusting the complex dielectric constant and impedance matching, enhancing polarization loss capability, and through a unique nanoneedle-shaped structure Promote multiple reflections of electromagnetic waves.

Benefits of technology

The electromagnetic wave absorption performance of the minimum reflection loss -60.22dB and the maximum effective absorption bandwidth of 6.2GHz is achieved in the frequency range of 2–18GHz, maintaining the flexibility of the material and meeting the application needs of thin thickness and wide bands.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004993428950000011
    Figure HDA0004993428950000011
  • Figure HDA0004993428950000021
    Figure HDA0004993428950000021
  • Figure HDA0004993428950000022
    Figure HDA0004993428950000022
Patent Text Reader

Abstract

The invention belongs to the technical field of electromagnetic wave absorption, and discloses a nano needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies and a preparation method and application thereof. In the preparation process of the nano needle-shaped NiCo2S4, a large number of sulfur vacancies are introduced while vulcanization is performed through a high-temperature annealing step, so that the polarization loss capability of the material is enhanced. In addition, the material has a unique nanoneedle structure, so that multiple reflection behaviors of incident electromagnetic waves can be further promoted. In addition, electromagnetic parameters can be regulated and controlled by changing the concentration of the metal salt. The preparation method is simple, rapid and suitable for large-scale preparation, and when the sample filling amount is 10 wt%, the electromagnetic wave absorbing composite material with the excellent wave absorbing performance can be obtained. According to the composite material, when the matching thickness is 1.87 mm in the frequency range of 2-18 GHz, the minimum reflection loss can reach-60.22 dB, and the maximum effective absorption bandwidth can reach 6.2 GHz.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electromagnetic wave absorption, and specifically relates to a nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorption material containing sulfur vacancies, and a preparation method and application thereof. Background Art

[0002] With the advancement of communication technology, electromagnetic pollution is becoming more and more serious, interfering with the normal operation of electronic equipment and posing a threat to human health. Traditional absorbers are mostly powder or block, and their mechanical properties are poor after adding molding agents and curing. With the rapid development and widespread application of flexible electronic devices, flexible electromagnetic wave absorbing materials have been born.

[0003] Carbon cloth is a flexible self-supporting fabric woven from carbon fibers. It has the lightness, high conductivity and stability of carbon materials, making it an ideal substrate for flexible materials. However, its high conductivity and impedance mismatch will lead to electromagnetic wave reflection, greatly reducing the absorption performance. The introduction of secondary growth can effectively improve the absorption performance of carbon cloth.

[0004] Double transition metal sulfides have good electrochemical properties and adjustable structures, making them ideal modified materials. Sulfur has a lower electronegativity, a smaller band gap than oxygen, a stronger conductivity than oxides, and good dielectric loss capacity. In addition, the preparation cost of double transition metal sulfides is low and the morphology is adjustable.

[0005] Defects in materials, such as vacancies and impurity atoms, will cause uneven distribution of electron clouds of atoms near the defects, thereby generating local dipoles. When the material is in an external electromagnetic field, these dipoles will polarize. In a changing electromagnetic field, the dipoles repeatedly undergo polarization orientation processes. Due to the existence of resistance such as friction, energy loss will occur, that is, the energy of electromagnetic waves will be dissipated. The presence of a large number of defects in the material will enhance the material's ability to absorb electromagnetic waves. In transition metal sulfides, sulfur atoms are relatively easy to detach from the lattice to form vacancies. By rationally designing the material preparation process, sulfur vacancy defects can be effectively introduced, thereby enhancing the material's electromagnetic wave absorption performance.

[0006] Introducing material defects is an effective strategy to enhance electromagnetic wave absorption performance. Therefore, how to grow transition metal sulfides on the surface of carbon cloth, introduce vacancy defects and regulate the microstructure to improve the electromagnetic wave absorption performance of the material needs further exploration. Summary of the invention

[0007] In order to solve the shortcomings and deficiencies in the above-mentioned prior art, the primary purpose of the present invention is to provide a method for preparing a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies.

[0008] Another object of the present invention is to provide a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorption material containing sulfur vacancies prepared by the above-mentioned preparation method: a large number of sulfur vacancy defects are introduced during the preparation process of NiCo2S4, and the vacancies can act as dipole polarization centers in the electromagnetic field to enhance the polarization loss capacity of the material, and the unique nano-needle structure can effectively promote multiple reflections of the incident electromagnetic waves, and a large number of heterogeneous interfaces have strong interface polarization capabilities.

[0009] Another object of the present invention is to provide an application of the above-mentioned sulfur vacancy-containing nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material.

[0010] The purpose of the present invention is achieved through the following technical solutions:

[0011] A method for preparing a nano-acicular nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies comprises the following steps:

[0012] (1) placing carbon in a muffle furnace and heating it for surface activation to obtain activated carbon cloth;

[0013] (2) adding nickel salt, cobalt salt and urea to deionized water, and continuously stirring to obtain solution A;

[0014] (3) completely immersing the activated carbon cloth obtained in step (1) into solution A obtained in step (2) to obtain solution B;

[0015] (4) transferring solution B and the activated carbon cloth immersed therein to a hydrothermal reactor, heating and then maintaining the temperature for reaction, and after the reaction is completed, cooling the hydrothermal reactor to room temperature, taking out the carbon cloth, washing and drying, and obtaining a double transition metal oxide / carbon cloth;

[0016] (5) placing the double transition metal oxide / carbon cloth in a porcelain ark, and then placing it on one end of the exhaust port of a tubular furnace, and placing a sulfiding agent on the air inlet end of the tubular furnace, and calcining at a high temperature to obtain a nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies.

[0017] The heating in step (1) is to heat the mixture to 450° C. at a heating rate of 5° C. / min and then keep the mixture warm for 2 hours for surface activation. The nickel salt in step (2) is nickel nitrate hexahydrate and the cobalt salt is cobalt nitrate hexahydrate. The continuous stirring time is 15 minutes.

[0018] The soaking time in step (3) is 1 hour; the heating process in step (4) is to heat the temperature to 120°C at a heating rate of 2°C / min and then keep the temperature for reaction for 4 hours; the drying temperature is 60°C and the drying time is 12 hours.

[0019] The vulcanizing agent in step (5) is thioacetamide; the high-temperature calcination is carried out by heating the temperature to 550°C at a heating rate of 5°C / min, and then calcining for 2 hours at a temperature keeping constant.

[0020] The amounts of the nickel salt, cobalt salt, urea in step (2) and the thioacetamide in step (5) are 1.0-3.0 mmol, 2.0-6.0 mmol, 3.0-12.0 mmol and 10 mmol, respectively, more preferably 2.0 mmol, 4.0 mmol, 6.0 mmol and 10 mmol.

[0021] A nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared by the above-mentioned preparation method.

[0022] The nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies vertically grows nano-needle-shaped NiCo2S4 containing sulfur vacancies in situ on the carbon cloth. The composite material has a large number of sulfur vacancies and a large number of heterogeneous interfaces between the nano-needles and the carbon cloth.

[0023] The sulfur-vacancy-containing nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorption material has a minimum reflection loss of -60.22 dB and a maximum effective absorption bandwidth of 6.2 GHz in the frequency range of 2-18 GHz when the matching thickness is 1.87 mm.

[0024] The application of the above-mentioned sulfur vacancy-containing nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorption material in the field of electromagnetic wave absorption.

[0025] Principle of the present invention:

[0026] The present invention prepares a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite material through a hydrothermal reaction and a high-temperature annealing process. A high-temperature annealing process is designed for vulcanization. First, thioacetamide is thermally decomposed into hydrogen sulfide gas to vulcanize the oxide precursor. Subsequently, sufficient energy is provided for the migration of sulfur atoms in a high-temperature environment, making it easier to migrate, so that it can be separated from the lattice to form atomic vacancies. The nano-needle-shaped NiCo2S4 grown vertically in situ on the surface of the carbon cloth adjusts the complex dielectric constant of the carbon cloth and improves the impedance matching of the composite material; and a large number of sulfur vacancy defects in the material enhance the polarization loss capacity of electromagnetic waves. The nano-needle-shaped NiCo2S4 containing sulfur vacancies grows on the surface of the carbon cloth, introducing a large number of heterogeneous interfaces and having interface polarization. In addition, the nano-needle-shaped NiCo2S4 containing sulfur vacancies is uniformly and densely arranged, which can promote multiple reflections of the incident electromagnetic waves, extend the transmission path of the electromagnetic waves, and improve the absorption capacity.

[0027] Compared with the prior art, the present invention has the following advantages and effects:

[0028] (1) The present invention adopts a hydrothermal method and a high temperature annealing process for preparation. The carbon cloth material is a substrate with good flexibility, NiCo2S4 has excellent electrochemical properties, and the structure is controllable. The introduction of this component can effectively adjust the complex dielectric constant and impedance matching degree of the composite material.

[0029] (2) The present invention adopts an air oxidation method to obtain activated carbon cloth, which is pollution-free, environmentally friendly and convenient compared with acid treatment; the obtained nano-needle-shaped NiCo2S4 / carbon cloth composite material containing sulfur vacancies can maintain good flexibility and meet application requirements; the high-temperature annealing sulfurization process introduces a large number of sulfur vacancy defects, which enhances the polarization loss capacity of the material. In addition, the material has a unique nano-needle structure, which can further promote the multiple reflection behavior of the incident electromagnetic wave. In addition, the electromagnetic parameters can be regulated by changing the concentration of the metal salt. The preparation method is simple and fast, suitable for large-scale preparation, and when the sample filling amount is 10wt%, an electromagnetic wave absorption composite material with excellent wave absorption performance can be obtained. The composite material has excellent reflection loss (-60.22dB, f=13.90GHz, d=1.87mm) and excellent effective absorption bandwidth (6.20GHz, d=1.87mm) in the frequency range of 2-18GHz. The sulfur-vacancy-containing nano-needle-shaped NiCo2S4 / carbon cloth composite material of the present invention meets the requirements of thin thickness, strong absorption, and wide frequency band while maintaining flexibility, and has broad application prospects in the field of electromagnetic wave absorption.

[0030] (3) The preparation method of the present invention can adjust the complex dielectric constant and microscopic morphology by changing the content of nickel salt, cobalt salt and urea, and achieve optimal absorption performance in different frequency bands.

[0031] (4) The preparation method of the present invention has few steps, short time, large output, is simple and convenient, and can achieve excellent electromagnetic wave absorption performance when the sample filling amount is only 10wt%. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is the scanning electron microscope image (ac) of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared in Examples 1 to 3.

[0033] Figure 2 It is the X-ray diffraction spectrum of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared in Examples 1 to 3.

[0034] Figure 3 This is a transmission electron microscope image of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared in Example 2.

[0035] Figure 4This is the electron paramagnetic resonance spectrum of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared in Example 2.

[0036] Figure 5 It is a three-dimensional graph (a–c) of the electromagnetic wave absorption performance of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorption material containing sulfur vacancies prepared in Examples 1 to 3 in the frequency range of 2–18 GHz.

[0037] Figure 6 It is the maximum effective absorption bandwidth (a–c) of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite material containing sulfur vacancies prepared in Examples 1 to 3 in the frequency range of 2–18 GHz.

[0038] Figure 7 Graph showing the electromagnetic wave attenuation constant of the sulfur vacancy-containing nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material prepared in Examples 1 to 3 in the frequency range of 2-18 GHz. DETAILED DESCRIPTION

[0039] The present invention is further described below with reference to specific embodiments, but they should not be construed as limiting the present invention.

[0040] Example 1: Preparation of NCS / CC-1 composite material

[0041] (1) placing the carbon cloth in a muffle furnace, heating it to 450°C at a heating rate of 5°C / min, and then keeping it at that temperature for 2 hours for surface activation to obtain an activated carbon cloth;

[0042] (2) adding 1 mmol nickel nitrate hexahydrate, 2 mmol nickel nitrate hexahydrate and 3 mmol urea to 50 mL deionized water and stirring for 15 minutes to obtain solution A;

[0043] (3) completely immersing the activated carbon cloth obtained in step (1) into solution A obtained in step (2) for 1 hour to obtain solution B;

[0044] (4) transferring solution B together with the activated carbon cloth immersed therein to a hydrothermal reactor, heating the solution to 120°C at a heating rate of 2°C / min, and then keeping the temperature for 4 hours. After the reaction is completed, the reactor is cooled to room temperature, the carbon cloth is taken out, washed, and dried at 60°C for 12 hours to obtain a double transition metal oxide / carbon cloth;

[0045] (5) The double transition metal oxide / carbon cloth was placed in a porcelain ark, and then placed at one end of the exhaust port of a tube furnace, and 10 mmol of thioacetamide was placed at the air inlet end of the tube furnace. The temperature was raised to 550°C at a heating rate of 5°C / min, and then kept warm for 2 hours to obtain a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies, which was named NCS / CC-1 composite material.

[0046] Example 2: Preparation of NCS / CC-2 composite material

[0047] (1) placing the carbon cloth in a muffle furnace, heating it to 450°C at a heating rate of 5°C / min, and then keeping it at that temperature for 2 hours for surface activation to obtain an activated carbon cloth;

[0048] (2) adding 2 mmol nickel nitrate hexahydrate, 4 mmol nickel nitrate hexahydrate and 6 mmol urea to 50 mL deionized water and stirring for 15 minutes to obtain solution A;

[0049] (3) completely immersing the activated carbon cloth obtained in step (1) into solution A obtained in step (2) for 1 hour to obtain solution B;

[0050] (4) transferring solution B together with the activated carbon cloth immersed therein to a hydrothermal reactor, heating the solution to 120°C at a heating rate of 2°C / min, and then keeping the temperature for 4 hours. After the reaction is completed, the reactor is cooled to room temperature, the carbon cloth is taken out, washed, and dried at 60°C for 12 hours to obtain a double transition metal oxide / carbon cloth;

[0051] (5) The double transition metal oxide / carbon cloth was placed in a porcelain ark, and then placed at one end of the exhaust port of a tube furnace, and 10 mmol of thioacetamide was placed at the air inlet end of the tube furnace. The temperature was raised to 550°C at a heating rate of 5°C / min, and then kept warm for 2 hours to obtain a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies, which was named NCS / CC-2 composite material.

[0052] Example 3: Preparation of NCS / CC-3 composite material

[0053] (1) placing the carbon cloth in a muffle furnace, heating it to 450°C at a heating rate of 5°C / min, and then keeping it at that temperature for 2 hours for surface activation to obtain an activated carbon cloth;

[0054] (2) 3 mmol nickel nitrate hexahydrate, 6 mmol nickel nitrate hexahydrate and 12 mmol urea were added to 50 mL deionized water and stirred for 15 minutes to obtain solution A;

[0055] (3) completely immersing the activated carbon cloth obtained in step (1) into solution A obtained in step (2) for 1 hour to obtain solution B;

[0056] (4) transferring solution B together with the activated carbon cloth immersed therein to a hydrothermal reactor, heating the solution to 120°C at a heating rate of 2°C / min, and then keeping the temperature for 4 hours. After the reaction is completed, the reactor is cooled to room temperature, the carbon cloth is taken out, washed, and dried at 60°C for 12 hours to obtain a double transition metal oxide / carbon cloth;

[0057] (5) The double transition metal oxide / carbon cloth was placed in a porcelain ark, and then placed at one end of the exhaust port of a tube furnace, and 10 mmol of thioacetamide was placed at the air inlet end of the tube furnace. The temperature was raised to 550°C at a heating rate of 5°C / min, and then kept warm for 2 hours to obtain a nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies, which was named NCS / CC-3 composite material.

[0058] Embodiment 4 (Effect Embodiment):

[0059] Structural characterization and performance testing of nano-needle nickel cobalt sulfide (NiCo2S4) / carbon cloth composite electromagnetic wave absorption materials containing sulfur vacancies:

[0060] (1) Composite material structure characterization:

[0061] The surface morphology of the sulfur vacancy-containing nano-needle-shaped nickel cobalt sulfide (NiCo2S4) / carbon cloth composite material prepared in Example 1-3 is as follows: Figure 1 As shown. The NiCo2S4 growth appears dense and uniform nanowires extending vertically outward from the carbon cloth fiber surface. Example 1 ( Figure 1 a), Example 2 ( Figure 1 b), Example 3 ( Figure 1 c) The microstructure remains consistent, but the length of the nanowires increases with the increase of metal salt concentration, indicating that the microstructure is controllable.

[0062] In order to characterize the crystal structure and composition of the nano-needle NiCo2S4 / carbon cloth composite material containing sulfur vacancies, X-ray diffraction analysis was performed on the product samples obtained in Examples 1 to 3. Figure 2As shown, two diffraction peaks can be observed for all samples at 25.6° and 43.7°, corresponding to the (002) and (101) crystal planes of graphite (JCPDS No.41-1487). In the embodiment, the main diffraction peaks associated with the (220), (311), (400), (511) and (440) crystal planes can be clearly observed at 26.8°, 31.6°, 38.3°, 50.4° and 55.3°. The matching with the standard diffraction pattern (JCPDS No.20-0728) verifies the successful synthesis of NiCo2S4. As the concentration of metal salt increases, the intensity of the two peaks of carbon cloth at 25.6° and 43.7° decreases. This is because the thickness of the nano-needle NiCo2S4 increases, affecting the peak signal of the carbon fiber.

[0063] In the TEM test, the spacing of the lattice fringes under high-resolution TEM is 0.164nm, 0.235nm and 0.280nm, which correspond to the (440), (400) and (311) crystal planes of NiCo2S4, respectively, proving the successful synthesis of NiCo2S4. In addition, point defects can be seen at the lattice fringes.

[0064] The electron paramagnetic resonance test of Example 1 shows an obvious electron paramagnetic resonance signal, which proves the existence of vacancies. The g value is calculated to be 2.003, and the vacancy type corresponding to the g value is sulfur vacancy. By comparing the carbon cloth sample, it can be proved that the vacancy originates from the grown NiCo2S4, and the successful introduction of sulfur vacancies is also proved.

[0065] (2) Performance characterization:

[0066] In order to evaluate the absorption performance of the nano-needle NiCo2S4 / carbon cloth composite material containing sulfur vacancies, its reflection loss value can be calculated according to the transmission line theory. 10% NiCo2S4 / carbon cloth composite material and 90% paraffin were prepared into a ring and tested by a vector network instrument. Figure 5 and Figure 6 The 3D reflection loss performance of Example 1, Example 2, and Example 3 when the thickness is 1-5 mm and the frequency is 2-18 GHz is shown. Figure 3 and Figure 4 , the minimum reflection loss of Example 1 is -37.16dB (2.89mm), and the effective bandwidth is 5.85GHz (1.66mm). Figure 5 b and Figure 6 b, the absorption performance of Example 2 is the best, the minimum reflection loss is -60.22dB, the corresponding thickness is 1.87mm, and the effective bandwidth is 6.20GHz. Figure 5 C and Figure 6The minimum reflection loss of Example 3 at 1.68 mm is -44.14 dB, and the effective bandwidth at 1.62 mm is 5.99 GHz. The results show that the absorption performance can be adjusted by adjusting the concentration of the metal salt in the solution. Example 2 achieves excellent absorption performance with low filler content and thin matching thickness.

[0067] The attenuation constant characterizes the composite material's ability to attenuate electromagnetic waves. Figure 7 As shown, in the frequency range of 2-18 GHz, the attenuation constant of Example 1 is the highest, indicating a stronger ability to resist electromagnetic wave loss. According to calculations, the average values ​​of the attenuation constants of Example 1, Example 2, and Example 3 are 176, 144, and 140, respectively. However, the impedance matching degree of Example 2 is better, and the electromagnetic wave can enter the interior of the material to a greater extent, so it exhibits the best performance.

[0068] The above is a detailed description of the preparation of sulfur vacancy-containing nanoneedle-shaped NiCo2S4 / carbon cloth composite electromagnetic wave absorption materials (NCS / CC-1, NCS / CC-2 and NCS / CC-3) through a hydrothermal method and a high-temperature annealing process.

[0069] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a nano-acicular nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies, characterized in that The following steps are involved: (1) placing carbon in a muffle furnace and heating it for surface activation to obtain activated carbon cloth; (2) adding nickel salt, cobalt salt and urea to deionized water, and continuously stirring to obtain solution A; (3) completely immersing the activated carbon cloth obtained in step (1) into the solution A obtained in step (2) to obtain a solution B; (4) transferring solution B and the activated carbon cloth immersed therein to a hydrothermal reactor, heating and then maintaining the temperature for reaction, and after the reaction is completed, cooling the hydrothermal reactor to room temperature, taking out the carbon cloth, washing and drying, and obtaining a double transition metal oxide / carbon cloth; (5) placing the double transition metal oxide / carbon cloth in a porcelain ark, and then placing it on one end of the exhaust port of a tubular furnace, and placing a sulfiding agent on the air inlet end of the tubular furnace, and calcining at a high temperature to obtain a nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies.

2. The method for preparing a nano-acicular nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 1, characterized in that: The heating in step (1) is to heat the mixture to 450° C. at a heating rate of 5° C. / min and then keep the mixture warm for 2 hours for surface activation. The nickel salt in step (2) is nickel nitrate hexahydrate and the cobalt salt is cobalt nitrate hexahydrate. The continuous stirring time is 15 minutes.

3. The method for preparing a nano-acrystal nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 1, characterized in that: The soaking time in step (3) is 1 hour; the heating process in step (4) is to heat the temperature to 120°C at a heating rate of 2°C / min and then keep the temperature for reaction for 4 hours; the drying temperature is 60°C and the drying time is 12 hours.

4. The method for preparing a nano-acicular nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 1, characterized in that: The vulcanizing agent in step (5) is thioacetamide; the high-temperature calcination is carried out by heating the temperature to 550°C at a heating rate of 5°C / min, and then calcining for 2 hours at a temperature keeping constant.

5. The method for preparing a nano-acicular nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 1, characterized in that: The amounts of the nickel salt, cobalt salt, urea in step (2) and the thioacetamide in step (5) are 1.0-3.0 mmol, 2.0-6.0 mmol, 3.0-12.0 mmol and 10 mmol, respectively.

6. The method for preparing a nano-acicular nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 1, characterized in that: The amounts of the nickel salt, cobalt salt, urea in step (2) and the thioacetamide in step (5) are 2.0 mmol, 4.0 mmol, 6.0 mmol and 10 mmol, respectively.

7. A nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies prepared by the preparation method according to any one of claims 1 to 6.

8. The nano-acrystal nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 7, characterized in that: The material vertically grows nano-needle-shaped NiCo2S4 containing sulfur vacancies in situ on carbon cloth.

9. The nano-acrystal nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorbing material containing sulfur vacancies according to claim 7, characterized in that: In the frequency range of 2–18 GHz, when the matching thickness is 1.87 mm, the minimum reflection loss of this material can reach -60.22 dB and the maximum effective absorption bandwidth can reach 6.2 GHz.

10. Use of the nano-needle-shaped nickel-cobalt sulfide / carbon cloth composite electromagnetic wave absorption material containing sulfur vacancies according to claim 7 in the field of electromagnetic wave absorption.