Hot-pressing thermal-deformation double-phase composite magnet and preparation method thereof
Through the preparation method of hot-pressed and hot-deformed dual-phase composite magnet, combined with induction + arc smelting, high-speed fast quenching, primary annealing, magnetic powder presintering and secondary annealing steps, the problems of large coercive force and easy cracking of hot-pressed and hot-deformed magnets are solved. , realizes magnet performance with high residual magnetism, low coercivity and high stability, and is suitable for power electronic devices.
Patent Information
- Application Number
- CN202411372622.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-26
AI Technical Summary
The existing hot-pressed and hot-deformed magnets have a large coercive force and are prone to cracking, making it difficult to meet the performance requirements of power electronic devices for high residual magnetism and low coercive dual-phase composite magnetic materials.
The preparation method of hot-pressed and hot-deformed biphasic composite magnet is prepared by induction + arc smelting, high-speed fast quenching, primary annealing, magnetic powder presintering, hot-pressed and hot-deforming and secondary annealing, and the rare earth element content is prepared at 3.5%~ 4% hot pressing and hot deformation of the biphasic composite magnet reduces the coercive force of the hard magnetic phase and increases the residual magnetism, and the low melting point element acts as a lubricant to prevent cracking.
Achieves high residual magnetism, low coercivity and high stability, thermally pressed and thermally deformed double-phase composite magnets, meet the magnetic performance requirements of power electronic devices such as permanent magnet contactors, transformers, circuit breakers, and solves the thermal pressure of magnets. Cracking problems during thermal deformation.
Smart Images

Figure CN119028686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic materials, and in particular to a hot pressing and hot deformation two-phase composite magnet and a preparation method thereof. Background Art
[0002] Due to the exchange coupling between nano-grains, the dual-phase composite magnetic material has both the high magnetic anisotropy and high coercivity of the hard magnetic phase and the high saturation magnetization intensity of the soft magnetic phase. The theoretical magnetic energy product (BH) max Up to 1MJ / m 3 , which is about twice that of single-phase NdFeB (the material with the highest existing magnetic energy product). At the same time, due to its low rare earth content, it has the characteristics of low cost, high temperature stability, excellent heat resistance and oxidation resistance.
[0003] Compared with single-phase NdFeB, the remanence of dual-phase composite magnetic materials is higher, but the coercive force is slightly lower. While magnetization can provide a large constant magnetic field to the outside, it only consumes less energy to complete rapid demagnetization, and realizes the rapid conversion of soft and hard magnetic phase magnetic properties. Based on this excellent magnetization and demagnetization characteristics, dual-phase composite magnetic materials have broad application prospects in power electronic devices such as permanent magnetic contactors, transformers, circuit breakers, and reactors.
[0004] In recent years, with the continuous development of new component systems and the deepening of theoretical research, the development of high remanence and low coercivity dual-phase composite magnetic materials has achieved many excellent results, but the coercivity is generally above 1000Oe, resulting in a large amount of energy required for charging and demagnetization, which is difficult to meet the performance requirements of power electronic devices for high remanence and low coercivity dual-phase composite magnetic materials. In addition, in order to meet the shape requirements of the material in practical applications, the material needs to be further processed into a bonded magnet or a hot-pressed and hot-deformed magnet. Among them, the bonded magnet has low remanence and coercivity due to the addition of non-magnetic binders. The hot-pressed and hot-deformed magnet has a higher magnet density and is superior to the bonded magnet in terms of magnetic properties. However, during the preparation process of the hot-pressed and hot-deformed magnet, it is very easy to induce shape anisotropy in the material, resulting in an increase in remanence and coercivity. At the same time, under the action of pressure, the hot-pressed and hot-deformed magnet also has the problem of easy cracking. Summary of the invention
[0005] In view of the problems of large coercive force and easy cracking of the above-mentioned existing hot-pressed and hot-deformed magnets, the present invention provides a hot-pressed and hot-deformed two-phase composite magnet and a preparation method thereof. The hot-pressed and hot-deformed two-phase composite magnet of the present invention has the advantages of high remanence, low coercive force, high stability, etc., and is conducive to application in power electronic devices such as permanent magnet contactors, transformers, circuit breakers, and reactors.
[0006] The present invention is achieved through the following technical solutions:
[0007] A hot pressing and hot deformation two-phase composite magnet, the general formula of the hot pressing and hot deformation two-phase composite magnet is: (RE a Nd 1-a ) b (Fe 1-c Co c ) 94-b-d-e B6M d T e ;
[0008] Among them, RE is a light rare earth element, M is a nucleation element, and T is a low melting point element;
[0009] a and c represent the molar fractions of RE and Co replacing Nd and Fe elements, respectively, satisfying 0≤a≤0.2 and 0≤c≤0.1;
[0010] b, d, and e represent the molar fractions of the total content of Nd and light rare earth elements, nucleation elements, and low melting point elements, respectively, satisfying 3.5≤b≤4, 0≤d≤1, and 0≤e≤2.
[0011] Furthermore, the light rare earth element RE is one or two of La, Ce and Y;
[0012] And / or, the nucleation element M is one or two of Cu, Cr, Nb and Zr;
[0013] And / or, the low melting point element T is one or two of In, Ga and Al.
[0014] A method for preparing a hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0015] According to the general structural formula of the hot-pressed and hot-deformed two-phase composite magnet, raw materials are weighed, and the raw materials are smelted several times under a protective atmosphere to obtain a uniformly smelted alloy ingot;
[0016] After the alloy ingot is crushed, it is heated to a molten state under a protective atmosphere, and the resulting melt is overflowed onto a cooling roller to form an amorphous phase thin ribbon;
[0017] The amorphous phase thin ribbon is subjected to an annealing treatment under vacuum conditions to obtain a nanometer dual-phase composite magnetic ribbon;
[0018] The nanometer dual-phase composite magnetic strip is powdered and sieved to obtain nanometer magnetic powder, the nanometer magnetic powder is pressed into a shape, and then pre-sintered under vacuum conditions to obtain a pre-sintered dual-phase composite magnet;
[0019] The pre-sintered two-phase composite magnet is pressurized and sintered under vacuum conditions to obtain a hot-pressed and hot-deformed magnet;
[0020] The hot pressed and hot deformed magnet is subjected to secondary annealing treatment under vacuum conditions to obtain a hot pressed and hot deformed two-phase composite magnet.
[0021] Furthermore, the raw materials are melted several times under a protective atmosphere, specifically: in an argon atmosphere, light rare earth elements RE, Nd, B and low melting point elements T are placed at the bottom, Fe, Co and nucleation elements M are placed at the top, and the bottom raw materials are melted by an induction coil while the top raw materials are melted by a 50-100A current arc, and the melting is performed 4-6 times.
[0022] Furthermore, the thickness of the amorphous phase thin strip is 15 to 30 μm, the width is 5 to 10 mm, and the rotation speed of the cooling roller is 20 to 50 m / s.
[0023] Furthermore, the amorphous phase thin strip is subjected to an annealing treatment under vacuum conditions, specifically: the amorphous phase thin strip is wrapped with a high thermal conductivity material and then sealed in a reaction container filled with protective gas, and an annealing treatment is performed under a vacuum environment. The annealing treatment is specifically: heating to 500-700°C at a heating rate of 1-5°C / min and keeping warm for 5-10 minutes.
[0024] Furthermore, the screening is specifically through a 120-mesh sieve, and the pressure of the pressing molding is 10-20 MPa.
[0025] Furthermore, the pre-sintering temperature is 700° C. to 1000° C., and the temperature is kept for 1 to 5 minutes.
[0026] Furthermore, the pre-sintered two-phase composite magnet is pressurized and sintered under vacuum conditions to obtain a hot pressed and hot deformed magnet, specifically: vacuuming to 1×10 -3 Pa or less, at 500-700°C, a pressure of 50-100 MPa is applied to the pre-sintered two-phase composite magnet, and it is taken out after 2-5 minutes to obtain a hot pressed and hot deformed magnet.
[0027] Furthermore, the hot pressed and heat deformed magnet is heated under vacuum conditions for secondary annealing, specifically: the hot pressed and heat deformed magnet is placed in a vacuum environment, heated to 400°C to 500°C at a heating rate of 1 to 5°C / min, and kept warm for 5 to 10 minutes.
[0028] Compared with the prior art, the present invention has the following beneficial technical effects:
[0029] The present invention is a hot-pressed and hot-deformed dual-phase composite magnet, wherein the rare earth element content is in the range of 3.5% to 4%, which is much lower than RE2Fe 14 The rare earth content in the B hard magnetic phase is 11.76%. The low light rare earth element content can reduce the high coercivity RE2Fe 14The B hard magnetic phase is generated, which indirectly increases the content of the soft magnetic phase with high saturation magnetic induction intensity, thereby increasing the remanence and reducing the coercive force. In addition, the addition of the ferromagnetic element Co can improve the ferromagnetic coupling between the element and the Fe element, which is beneficial to improving the remanence of the magnetic phase. The addition of a small amount of nucleation element M can serve as a non-uniform nucleation point of the magnetic phase to increase its nucleation power, promote the precipitation and refinement of the soft and hard magnetic phases, and help to improve the exchange coupling between the soft and hard magnetic phases, thereby achieving the effect of improving the remanence of the material. The addition of the low melting point element T is beneficial to the magnet as a lubricant during the hot pressing and hot deformation process to promote the rotation of the soft and hard magnetic phase grains and prevent the magnet from cracking.
[0030] Furthermore, replacing part of the Nd element with one or two of the light rare earth elements La, Ce, and Y, with a replacement ratio between 0 and 20%, will significantly reduce RE2Fe 14 The anisotropy field of the hard magnetic phase (Y2Fe 14 B. La2Fe 14 B. Ce2Fe 14 The anisotropy field of B is much smaller than that of Nd2Fe 14 B) by reducing the coercivity of the hard magnetic phase to reduce the coercivity of the magnet as a whole.
[0031] In the preparation method of the hot pressing and hot deformation dual-phase composite magnet of the present invention, magnetic powder pre-sintering and secondary annealing steps are respectively added before and after the hot pressing and hot deformation process. During the pre-sintering process of the magnetic powder, part of the magnetic powder is solidified, which can improve its mechanical strength and reduce deformation and cracking during the hot pressing and hot deformation process. The secondary annealing can eliminate the residual internal stress of the magnet during the hot pressing and hot deformation process, thereby reducing the coercive force, thereby meeting the magnetic property requirements of the high remanence and low coercive force hot pressing and hot deformation dual-phase composite magnet for power electronic devices such as permanent magnetic contactors, transformers, circuit breakers, and reactors. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a microscopic morphology of the hot pressed and hot deformed two-phase composite magnet of Example 7.
[0033] Figure 2 It is the microscopic morphology of the hot pressed and hot deformed two-phase composite magnet of the comparative example. DETAILED DESCRIPTION
[0034] The present invention is described in detail below:
[0035] The present invention provides a hot pressing and hot deformation two-phase composite magnet, the general formula of which is: (RE a Nd 1-a ) b (Fe 1-c Co c ) 94-b-d- e B6Md T e ; Wherein, RE is a light rare earth element, M is a nucleation element, and T is a low melting point element; a and c represent the molar fractions of RE and Co replacing Nd and Fe elements, respectively, satisfying 0≤a≤0.2, 0≤c≤0.1; b, d, and e represent the molar fractions of the total content of Nd and light rare earth elements, nucleation elements, and low melting point elements, respectively, satisfying 3.5≤b≤4, 0≤d≤1, and 0≤e≤2.
[0036] The light rare earth element RE is one or two of La, Ce and Y.
[0037] The nucleation element M is one or two of Cu, Cr, Nb and Zr.
[0038] The low melting point element T is one or two of In, Ga and Al.
[0039] The present invention also provides a method for preparing the above-mentioned hot pressing and hot deformation two-phase composite magnet, comprising six steps: ① induction + arc melting, ② high-speed rapid quenching, ③ primary annealing, ④ magnetic powder pre-sintering, ⑤ hot pressing and hot deformation, and ⑥ secondary annealing.
[0040] The specific process of the induction + arc melting is as follows: weigh and proportion the light rare earth elements RE, Nd, Fe, Co, B, nucleation elements M, and low melting point elements T according to the atomic percentages described in the general formula above, put the weighed raw materials into the crucible of the vacuum melting furnace, put the rare earth elements RE, B, and low melting point elements T at the bottom of the crucible, and put other high melting point elements at the top of the crucible. While heating and melting the bottom raw materials with an induction coil under the protection of an argon atmosphere, a 50-100A high current arc is used at the top for local high temperature melting. In this way, the induction and arc melting are combined for 4-6 times to obtain a uniformly melted alloy ingot. The combination of induction melting and arc melting can, on the one hand, promote the full melting and bonding of the raw materials to form an alloy ingot with uniform composition distribution, and on the other hand, prevent the transitional volatilization of low melting point elements from causing the alloy ingot to differ too much from the theoretical composition.
[0041] The specific process of the high-speed quenching step ② is as follows: the alloy ingot obtained in step ① is broken into small pieces, and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy fragments in the quartz tube are reheated to a molten state, and then the resulting melt is overflowed onto a cooling copper roller with a rotation rate of 20 to 50 m / s to form an amorphous phase thin strip with a thickness of 15 to 30 μm and a width of 5 to 10 mm.
[0042] The specific process of the first annealing in step ③ is: wrap the amorphous phase ribbon formed in step ② with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a vacuum heat treatment furnace, raise the furnace temperature to 500-700℃ at a heating rate of 1-5℃ / min, and keep it warm for 5-10min. The use of high thermal conductivity quartz wool wrapping and an ultra-low heating rate of 1-5℃ / min can ensure that the amorphous phase ribbon remains heated evenly during the heating process, avoiding abnormal precipitation of nano-grains due to uneven heating. The lower heat treatment temperature of 500-700℃ and the short insulation time of 5-10min are not only conducive to the smooth precipitation of nano-grains of soft and hard magnetic phases from the amorphous phase ribbon, but also improve the nano exchange coupling effect between soft and hard magnetic phase grains, improve the remanence, and avoid the problem of abnormal growth of grains due to excessively high heat treatment temperature and excessively long insulation time, thereby weakening the exchange coupling effect. After the heat preservation is completed, the quartz tube containing the amorphous phase ribbon is quickly placed in cold water to cool to room temperature to prevent the soft and hard magnetic phase grains in the amorphous phase ribbon from growing slowly during the cooling process of the ribbon, thereby obtaining a nanometer dual-phase composite magnetic ribbon.
[0043] The specific process of the ④ magnetic powder pre-sintering is as follows: the nano two-phase composite magnetic strip obtained in step ③ is mechanically ground into powder, passed through a 120-mesh sieve, and nano magnetic powder with basically uniform particle size is obtained. The nano magnetic powder is loaded into a mold, formed under a pressure of 10 to 20 MPa, and then placed in a vacuum sintering furnace for pre-sintering (700°C to 1000°C for 1 to 5 minutes) to obtain a pre-sintered two-phase composite magnet. A higher sintering temperature can solidify part of the magnetic powder, improve its mechanical strength, and reduce deformation and cracking during hot pressing and thermal deformation, while a short-term insulation of 1 to 5 minutes can prevent the nano grains from growing further during the pre-sintering process.
[0044] The specific process of hot pressing and thermal deformation in step ⑤ is as follows: the pre-sintered two-phase composite magnet obtained in step ④ is reloaded into the mold, placed in an electric field assisted hot pressing sintering furnace, and vacuumed to 1×10 -3 Pa, at 500-700℃, a pressure of 50-100MPa is applied to the pre-sintered two-phase composite magnet, and it is taken out after 2-5min to obtain a hot pressed and hot deformed magnet. After hot pressing and hot deformation at 500℃-700℃ and 50-100MPa, the density of the hot pressed and hot deformed magnet is greatly improved compared with the pre-sintered two-phase composite magnet, and the remanence and coercive force are significantly improved.
[0045] The specific process of the secondary annealing in step ⑥ is as follows: the hot pressed and hot deformed magnet obtained in step ⑤ is placed in a vacuum heat treatment furnace, and a secondary annealing treatment is performed at a temperature of 400°C to 500°C at a heating rate of 1 to 5°C / min, and the temperature is kept for 5 to 10 minutes to eliminate the residual internal stress of the hot pressed and hot deformed magnet during the hot pressing and hot deformation process, reduce the coercive force, and obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercive force.
[0046] The embodiments of the present invention will be described in detail below in conjunction with the examples. The implementation cases are preferred embodiments of the present invention and should not be used to limit the scope of the present invention. In the following examples, the methods and experimental equipment used are all conventional methods and instruments unless otherwise specified.
[0047] Example 1
[0048] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by the chemical formula Nd 3.5 Fe 90.5 B6.
[0049] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0050] ① Induction + arc melting: weigh and proportion the light rare earth elements Nd, Fe, and B according to the atomic percentages described in the general formula above, put the weighed raw materials into the crucible of the vacuum melting furnace, put the Nd and B elements at the bottom of the crucible, and put the Fe element at the top of the crucible. While heating the bottom raw materials with an induction coil under the protection of an argon atmosphere, a 50A arc is used on the top for local high-temperature melting. This induction and arc combination melting is repeated 6 times to obtain a uniformly melted alloy ingot;
[0051] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation rate of 50m / s to form an amorphous phase thin strip with a thickness of 15μm and a width of 10mm;
[0052] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, raise the furnace temperature to 700°C at a heating rate of 5°C / min, and keep it warm for 5 minutes. After the insulation is completed, the quartz tube containing the ribbon is quickly placed in cold water to cool to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0053] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 10MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 1000℃ and a holding time of 1min to obtain a pre-sintered dual-phase composite magnet.
[0054] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3Pa, a hot pressing and hot deformation treatment was carried out at a temperature of 625°C and a pressure of 90 MPa, and maintained for 3 minutes to obtain a hot pressed and hot deformed magnet.
[0055] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 500°C at a heating rate of 5°C / min, and keep it warm for 5 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0056] Example 2
[0057] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by a chemical formula (La 0.1 Y 0.1 Nd 0.8 )4Fe 90 B6.
[0058] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0059] ① Induction + arc melting: weigh and proportion the light rare earth elements La, Y, Nd, Fe, and B according to the atomic percentages described in the general formula above, put the weighed raw materials into a crucible of a vacuum melting furnace, put La, Y, Nd, and B elements at the bottom of the crucible, and put Fe element at the top of the crucible. While heating the bottom raw materials with an induction coil under the protection of an argon atmosphere, use a 50A arc to perform local high-temperature melting 6 times on the top to obtain a uniformly smelted alloy ingot;
[0060] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation rate of 20m / s to form an amorphous phase thin strip with a thickness of 30μm and a width of 5mm;
[0061] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 500°C at a heating rate of 1°C / min and keep it warm for 10 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0062] ④ Magnetic powder pre-sintering: The nanometer dual-phase composite magnetic strip is mechanically ground into powder, and passed through a 120-mesh sieve to obtain nanometer magnetic powder with basically uniform particle size. The nanometer magnetic powder is loaded into a mold, formed under a pressure of 20MPa, and then placed in a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 700℃ and a holding time of 5min to obtain a pre-sintered dual-phase composite magnet.
[0063] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa or less, and hot pressing and hot deformation treatment is carried out at a temperature of 500°C and a pressure of 100 MPa, and maintained for 5 minutes to obtain a hot pressed and hot deformed magnet.
[0064] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 400°C at a heating rate of 1°C / min, and keep it warm for 10 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0065] Example 3
[0066] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by a chemical formula (Ce 0.2 Nd 0.8 )4Fe 90 B6.
[0067] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0068] ① Induction + arc melting: weigh and proportion the light rare earth elements Ce, Nd, Fe, and B according to the atomic percentage described in the above general formula, put the weighed raw materials into the crucible of the vacuum melting furnace, put Ce, Nd, and B elements at the bottom of the crucible, and put Fe element at the top of the crucible. While heating the bottom raw materials with an induction coil under the protection of argon atmosphere, use a 50A arc to perform local high-temperature melting 6 times on the top to obtain a uniformly smelted alloy ingot;
[0069] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation speed of 40m / s to form an amorphous phase thin strip with a thickness of 20μm and a width of 8mm;
[0070] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 650°C at a heating rate of 3°C / min and keep it warm for 6 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0071] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 15MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 850℃ and a holding time of 3min to obtain a pre-sintered dual-phase composite magnet.
[0072] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa or less, and hot pressing and hot deformation treatment is carried out at a temperature of 600°C and a pressure of 95MPa, and maintained for 4min to obtain a hot pressed and hot deformed magnet.
[0073] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 450°C at a heating rate of 3°C / min, and keep it warm for 6 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0074] Example 4
[0075] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by a chemical formula (La 0.1 Y 0.1 Nd 0.8 )4(Fe 0.9 Co 0.1 ) 88 B6 0.5 Nb 0.5 Al1.
[0076] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0077] ① Induction + arc melting: weigh and proportion the light rare earth elements La, Y, Nd, Fe, Co, B, Cu, Nb, and Al according to the atomic percentages described in the general formula above, put the weighed raw materials into a crucible of a vacuum melting furnace, put La, Y, Nd, B, and Al at the bottom of the crucible, and put Fe, Co, Cu, and Nb elements at the top of the crucible. While heating the bottom raw materials with an induction coil under the protection of an argon atmosphere, use a 100A arc at the top for local high-temperature melting 4 times to obtain a uniformly smelted alloy ingot;
[0078] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation rate of 20m / s to form an amorphous phase thin strip with a thickness of 30μm and a width of 10mm;
[0079] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 500°C at a heating rate of 1°C / min and keep it warm for 10 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0080] ④ Magnetic powder pre-sintering: The nanometer dual-phase composite magnetic strip is mechanically ground into powder, and passed through a 120-mesh sieve to obtain nanometer magnetic powder with basically uniform particle size. The nanometer magnetic powder is loaded into a mold, formed under a pressure of 20MPa, and then placed in a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 700℃ and a holding time of 5min to obtain a pre-sintered dual-phase composite magnet.
[0081] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa or less, and hot pressing and hot deformation treatment is carried out at a temperature of 500°C and a pressure of 100 MPa, and maintained for 5 minutes to obtain a hot pressed and hot deformed magnet.
[0082] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 400°C at a heating rate of 1°C / min, and keep it warm for 10 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0083] Example 5
[0084] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by a chemical formula (La 0.1 Y 0.1 Nd 0.8 )4(Fe 0.9 Co 0.1 ) 88 B6Cr 0.5 Zr 0.5 In1Ga1.
[0085] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0086] ① Induction + arc melting: La, Y, Nd, Fe, Co, B, Cr, Zr, In, and Ga are weighed and proportioned according to the atomic percentages described in the general formula above, and the weighed raw materials are placed in a crucible of a vacuum melting furnace, with La, Y, Nd, B, In, and Ga elements placed at the bottom of the crucible, and Fe, Co, Cr, and Zr elements placed at the top of the crucible. While the bottom raw materials are heated by an induction coil under the protection of an argon atmosphere, a 100A arc is used at the top for local high-temperature melting 4 times to obtain a uniformly smelted alloy ingot;
[0087] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation speed of 30m / s to form an amorphous phase thin strip with a thickness of 25μm and a width of 10mm;
[0088] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 600°C at a heating rate of 2°C / min and keep it warm for 8 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0089] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 20MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 800℃ and a holding time of 3min to obtain a pre-sintered dual-phase composite magnet.
[0090] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa or less, and hot pressing and hot deformation treatment is carried out at a temperature of 700°C and a pressure of 50MPa, and maintained for 2min to obtain a hot pressed and hot deformed magnet.
[0091] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 500°C at a heating rate of 5°C / min, and keep it warm for 5 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0092] Example 6
[0093] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by a chemical formula (La 0.1 Y 0.1 Nd 0.8 )4(Fe 0.9 Co 0.1 ) 88 B6Cu1In1Ga1.
[0094] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0095] ① Induction + arc melting: La, Y, Nd, Fe, Co, B, Cu, In, and Ga are weighed and proportioned according to the atomic percentages described in the general formula above, and the weighed raw materials are placed in a crucible of a vacuum melting furnace, with La, Y, Nd, B, In, and Ga elements placed at the bottom of the crucible, and Fe, Co, and Cu elements placed at the top of the crucible. While the bottom raw materials are heated by an induction coil under the protection of an argon atmosphere, a 100A arc is used at the top for local high-temperature melting 4 times to obtain a uniformly smelted alloy ingot;
[0096] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation speed of 30m / s to form an amorphous phase thin strip with a thickness of 25μm and a width of 10mm;
[0097] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 600°C at a heating rate of 2°C / min and keep it warm for 8 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0098] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 20MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 800℃ and a holding time of 3min to obtain a pre-sintered dual-phase composite magnet.
[0099] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa or less, and hot pressing and hot deformation treatment is carried out at a temperature of 700°C and a pressure of 50MPa, and maintained for 2min to obtain a hot pressed and hot deformed magnet.
[0100] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 500°C at a heating rate of 5°C / min, and keep it warm for 5 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0101] Example 7
[0102] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by the chemical formula Nd 3.5 Fe 89.5 B6Al1.
[0103] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0104] ① Induction + arc melting: Nd, Fe, B, and Al are weighed and proportioned according to the atomic percentages described in the general formula above, and the weighed raw materials are placed in a crucible of a vacuum melting furnace, with Nd, B, and Al elements placed at the bottom of the crucible and Fe element placed at the top of the crucible. While the bottom raw materials are heated by an induction coil under the protection of an argon atmosphere, a 60A arc is used at the top for local high-temperature melting for 5 times to obtain a uniformly melted alloy ingot;
[0105] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation rate of 50m / s to form an amorphous phase thin strip with a thickness of 15μm and a width of 10mm;
[0106] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, and then put it into a heat treatment furnace. Raise the furnace temperature to 700°C at a heating rate of 5°C / min and keep it warm for 5 minutes. After the insulation is completed, quickly put the quartz tube containing the ribbon into cold water to cool it to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0107] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 10MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 1000℃ and a holding time of 1min to obtain a pre-sintered dual-phase composite magnet.
[0108] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa, a hot pressing and hot deformation treatment was carried out at a temperature of 625°C and a pressure of 90 MPa, and maintained for 3 minutes to obtain a hot pressed and hot deformed magnet.
[0109] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 500°C at a heating rate of 5°C / min, and keep it warm for 5 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0110] Example 8
[0111] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by the chemical formula Nd4Fe 90 B6.
[0112] The method for preparing the hot pressing and hot deformation two-phase composite magnet comprises the following steps:
[0113] ① Induction + arc melting: weigh and proportion the light rare earth elements Nd, Fe, and B according to the atomic percentages described in the general formula above, put the weighed raw materials into the crucible of the vacuum melting furnace, put the Nd and B elements at the bottom of the crucible, and put the Fe element at the top of the crucible. While heating the bottom raw materials with an induction coil under the protection of an argon atmosphere, a 50A arc is used on the top for local high-temperature melting. This induction and arc combination melting is repeated 6 times to obtain a uniformly melted alloy ingot;
[0114] ② High-speed quenching: The alloy ingot is broken into small pieces and placed in a quartz tube in a melt quenching furnace. After the melt quenching furnace is evacuated and high-purity argon is introduced, the alloy pieces in the quartz tube are reheated to a molten state, and then the melt is overflowed onto a cooling copper roller with a rotation rate of 50m / s to form an amorphous phase thin strip with a thickness of 15μm and a width of 10mm;
[0115] ③ Primary annealing: Wrap the amorphous ribbon with quartz wool, seal it in a quartz tube filled with argon gas, raise the furnace temperature to 700°C at a heating rate of 5°C / min, and keep it warm for 5 minutes. After the insulation is completed, the quartz tube containing the ribbon is quickly placed in cold water to cool to room temperature to obtain a nano dual-phase composite magnetic ribbon.
[0116] ④ Pre-sintering of magnetic powder: Grind the nanometer dual-phase composite magnetic strip into powder mechanically, pass it through a 120-mesh sieve, and obtain nanometer magnetic powder with basically uniform particle size. Put the nanometer magnetic powder into a mold, shape it under a pressure of 10MPa, and then put it into a vacuum sintering furnace for pre-sintering at a pre-sintering temperature of 1000℃ and a holding time of 1min to obtain a pre-sintered dual-phase composite magnet.
[0117] ⑤Hot pressing and thermal deformation: The pre-sintered two-phase composite magnet is reloaded into the mold and placed in an electric field assisted hot pressing sintering furnace, and the vacuum is evacuated to 1×10 -3 Pa, a hot pressing and hot deformation treatment was carried out at a temperature of 625°C and a pressure of 90 MPa, and maintained for 3 minutes to obtain a hot pressed and hot deformed magnet.
[0118] ⑥ Secondary annealing: Place the hot pressed and hot deformed magnet in a vacuum heat treatment furnace, heat it to 500°C at a heating rate of 5°C / min, and keep it warm for 5 minutes to obtain a hot pressed and hot deformed dual-phase composite magnet with high remanence and low coercivity.
[0119] Comparative Example
[0120] A hot pressed and hot deformed two-phase composite magnet, the composition and content of which are expressed by the chemical formula Nd 3.5 Fe 90.5 B6. The preparation method is similar to that of Specific Example 1. The difference is that the preparation process does not include step ④ pre-sintering of magnetic powder and step ⑥ secondary annealing.
[0121] The residual magnetic induction intensity B of the hot pressed and hot deformed magnets prepared in Examples 1 to 7 and the comparative example was measured by a vibrating sample magnetometer (VSM). r and coercivity H c , the test results are shown in Table 1.
[0122] Table 1 Magnetic properties test results of hot pressing and hot deformation dual-phase composite magnets
[0123] Group Element <![CDATA[B r (T)]]> <![CDATA[H c (You)]]> Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[Nd <h2 style=";text-align:left;direction:ltr"> 3.5 <h2 style=";text-align:left;direction:ltr"> Fe<h2 style=";text-align:left;direction:ltr"> 90.5 <h2 style=";text-align:left;direction:ltr"> B6]]><h2 style=";text-align:left;direction:ltr"> 0.52 396 Example 2 <![CDATA[(La 0.1 Y 0.1 Nd 0.8 )4Fe 90 B6]]> 0.49 356 Example 3 <![CDATA[(Ce 0.2 Nd 0.8 )4Fe 90 B6]]> 0.47 362 Example 4 <![CDATA[(La 0.1 Y 0.1 Nd 0.8 )4(Fe 0.9 Co 0.1 ) 88 B6Cu 0.5 Nb 0.5 Al1]]> 0.65 289 Example 5 <h2 style=";text-align:left;direction:ltr"><![CDATA[(La <h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> Y<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> Nd<h2 style=";text-align:left;direction:ltr"> 0.8 <h2 style=";text-align:left;direction:ltr"> )4(Fe<h2 style=";text-align:left;direction:ltr"> 0.9 <h2 style=";text-align:left;direction:ltr"> Co<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 88 <h2 style=";text-align:left;direction:ltr"> B6Cr<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> Zr<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> In1Ga1]]><h2 style=";text-align:left;direction:ltr"> 0.70 282 Example 6 <![CDATA[(La 0.1 Y 0.1 Nd 0.8 )4(Fe 0.9 Co 0.1 ) 88 B6Cu1In1Ga1]]> 0.63 302 Example 7 <![CDATA[Nd 3.5 Fairy 89.5 B6Al1]]> 0.50 401 Example 8 <![CDATA[Nd4Fe 90 B6]]> 0.47 407 Comparative Example <h2 style=";text-align:left;direction:ltr"><![CDATA[Nd <h2 style=";text-align:left;direction:ltr"> 3.5 <h2 style=";text-align:left;direction:ltr"> Fe<h2 style=";text-align:left;direction:ltr"> 90.5 <h2 style=";text-align:left;direction:ltr"> B6]]><h2 style=";text-align:left;direction:ltr"> 0.43 452
[0124] By comparing the magnetic performance parameters of the embodiment and the comparative example in Table 1, it can be seen that the hot pressing and hot deformation two-phase composite magnet prepared by the present invention has excellent high remanence and low coercivity characteristics, and the residual magnetic induction intensity B r Above 0.47T, the maximum can reach 0.70T, the coercive force H c By comparing the magnetic properties of Example 1 with that of Example 8, it is found that appropriately reducing the rare earth element content and increasing the Fe element content can effectively increase the remanence of the hot pressed and hot deformed dual-phase composite magnet and reduce the coercive force. r From the original 0.47T to 0.52T, H c The magnetic properties of Examples 2 and 3 are compared with those of Example 8. The results show that the use of light rare earth elements La, Y, and Ce to replace part of the Nd element is beneficial to reducing RE2Fe 14 The anisotropy field of the hard magnetic phase B reduces the coercivity from 407Oe to below 362Oe, while the remanence remains above 0.47T. By comparing the magnetic properties test results of Examples 2, 4, 5, 6 and 8, it can be seen that the addition of a small amount of ferromagnetic element Co and nucleation element M promotes the precipitation of the soft magnetic phase α-Fe, which is beneficial to improving the exchange coupling between the soft and hard magnetic phases, thereby achieving the effect of increasing the remanence of the material and reducing the coercivity. B r From 0.47T to over 0.49T, while H c The magnetic properties of the material are reduced from 407Oe to below 356Oe, and the best magnetic properties are B r =0.70T,H c =282Oe. By comparing the magnetic properties of Example 1 and the comparative example, it can be seen that after adding the magnetic powder pre-sintering and secondary annealing steps before and after hot pressing and hot deformation, the anisotropy of the magnet is weakened, making the remanence B r From 0.43T to 0.52T, the coercive force H c By comparing the magnetic properties of Example 7 with the comparative example, it is found that the addition of a small amount of low melting point element T will not reduce the magnetic properties of the magnet. r and coercivity H c They remain around 0.43T and 452Oe respectively.
[0125] In addition, the microstructures of Example 7 and the comparative example were measured by SEM. Figure 1 is the microscopic morphology of Example 7, Figure 2The microscopic morphology of the comparative example is shown in Figure 2. The results show that when the conventional hot pressing and hot deformation process is used to prepare hot pressing and hot deformation magnets, due to the lack of a low melting point phase as a lubricant, it is difficult for the magnet to reach a completely dense state, and there are many holes. These holes lead to a decrease in magnet density and poor magnetic properties. On this basis, after adding the steps of magnetic powder pre-sintering and secondary annealing (Example 1), and adding a small amount of low melting point elements (Example 7), the holes basically disappear (as shown in Figure 2). Figure 1 As shown in the figure, the magnet density increases, the remanence increases, and the coercive force decreases slightly. This shows that the addition of low melting point element T, the addition of magnetic powder pre-sintering and the secondary annealing steps can not only affect the magnetic properties of the magnet, but also solve the cracking problem of the dual-phase composite magnet during hot pressing and hot deformation, and improve the thermal stability.
[0126] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A hot pressing and hot deformation two-phase composite magnet, It is characterized in that The general formula of the hot pressing and hot deformation two-phase composite magnet is: (RE a Nd 1-a ) b (Fe 1-c Co c ) 94-b-d-e B 6 M d T e ; Among them, RE is a light rare earth element, M is a nucleation element, and T is a low melting point element; a and c represent the molar fractions of RE and Co replacing Nd and Fe elements, respectively, satisfying 0≤a≤0.2 and 0≤c≤0.1; b, d, and e represent the molar fractions of the total content of Nd and light rare earth elements, nucleation elements, and low melting point elements, respectively, satisfying 3.5≤b≤4, 0≤d≤1, and 0≤e≤2.
2. The hot pressing and hot deformation two-phase composite magnet according to claim 1, It is characterized in that The light rare earth element RE is one or two of La, Ce and Y; And / or, the nucleation element M is one or two of Cu, Cr, Nb and Zr; And / or, the low melting point element T is one or two of In, Ga and Al.
3. A method for preparing a hot pressing and hot deformation two-phase composite magnet according to claim 1 or 2, It is characterized in that The following steps are involved: According to the general structural formula of the hot-pressed and hot-deformed two-phase composite magnet, raw materials are weighed, and the raw materials are smelted several times under a protective atmosphere to obtain a uniformly smelted alloy ingot; After the alloy ingot is crushed, it is heated to a molten state under a protective atmosphere, and the resulting melt is overflowed onto a cooling roller to form an amorphous phase thin ribbon; The amorphous phase thin ribbon is subjected to an annealing treatment under vacuum conditions to obtain a nanometer dual-phase composite magnetic ribbon; The nanometer dual-phase composite magnetic strip is powdered and sieved to obtain nanometer magnetic powder, the nanometer magnetic powder is pressed into a shape, and then pre-sintered under vacuum conditions to obtain a pre-sintered dual-phase composite magnet; The pre-sintered two-phase composite magnet is pressurized and sintered under vacuum conditions to obtain a hot-pressed and hot-deformed magnet; The hot pressed and hot deformed magnet is subjected to secondary annealing treatment under vacuum conditions to obtain a hot pressed and hot deformed two-phase composite magnet.
4. The method for preparing a hot pressing and hot deformation dual-phase composite magnet according to claim 3, It is characterized in that The raw materials are melted several times under a protective atmosphere, specifically: in an argon atmosphere, light rare earth elements RE, Nd, B and low melting point elements T are placed at the bottom, Fe, Co and nucleation elements M are placed at the top, and an induction coil is used to melt the bottom raw materials while a 50-100A current arc is used to melt the top raw materials, and the melting is performed 4-6 times.
5. The method for preparing a hot pressing and hot deformation two-phase composite magnet according to claim 3, It is characterized in that The amorphous phase thin strip has a thickness of 15 to 30 μm and a width of 5 to 10 mm, and the rotation speed of the cooling roller is 20 to 50 m / s.
6. The method for preparing a hot pressing and hot deformation two-phase composite magnet according to claim 3, It is characterized in that The amorphous phase thin strip is subjected to an annealing treatment under vacuum conditions, specifically: the amorphous phase thin strip is wrapped with a high thermal conductivity material and then sealed in a reaction container filled with protective gas, and an annealing treatment is performed under a vacuum environment. The annealing treatment specifically comprises: heating the temperature to 500-700°C at a heating rate of 1-5°C / min and keeping the temperature for 5-10 minutes.
7. The method for preparing a hot pressing and hot deformation dual-phase composite magnet according to claim 3, It is characterized in that The screening is specifically through a 120-mesh sieve, and the pressure of the compression molding is 10-20 MPa.
8. The method for preparing a hot pressing and hot deformation dual-phase composite magnet according to claim 3, It is characterized in that The pre-sintering temperature is 700° C. to 1000° C., and the temperature is kept for 1 to 5 minutes.
9. The method for preparing a hot pressing and hot deformation dual-phase composite magnet according to claim 3, It is characterized in that The pre-sintered two-phase composite magnet is pressurized and sintered under vacuum to obtain a hot pressed and hot deformed magnet. Specifically, the vacuum is evacuated to 1×10 -3 Pa or less, at 500-700°C, a pressure of 50-100 MPa is applied to the pre-sintered two-phase composite magnet, and it is taken out after 2-5 minutes to obtain a hot pressed and hot deformed magnet.
10. The method for preparing a hot pressing and hot deformation two-phase composite magnet according to claim 3, It is characterized in that The hot pressed and heat deformed magnet is heated under vacuum conditions for secondary annealing, specifically: the hot pressed and heat deformed magnet is placed in a vacuum environment, heated to 400°C to 500°C at a heating rate of 1 to 5°C / min, and kept warm for 5 to 10 minutes.
Citation Information
Cited By
Microcrystal and nanocrystalline neodymium iron boron anisotropic magnetic powder with high permanent magnet performance and preparation method of microcrystal and nanocrystalline neodymium iron boron anisotropic magnetic powder
CN121938770A