Ceramic capacitor with MIM structure and production method
In the production of MIM structure capacitors, photoresist is used to form a raised module and sputter a metal layer to form a positive trapezoidal electrode, which solves the problem of uneven electrode etching caused by the wet etching process and improves product reliability and stability sex.
Patent Information
- Application Number
- CN202411166609.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
In the production process of MIM structure capacitors, due to the unselective nature of the wet engraving process, the etching of the electrodes is uneven, forming a cross-section similar to an inverted trapezoidal shape, affecting the reliability of the product.
By coating photoresist on the ceramic dielectric layer, a raised module is formed, and a metal layer is sputtered therebetween, forming a second metal layer in a positive trapezoidal shape, ensuring the stability and connection strength of the electrodes, and removing light in subsequent processes Resist and excess metal layer to avoid lateral erosion of the etching liquid.
It improves the reliability of the capacitor, ensures that the gold wire is not easy to tear off the edge of the second metal layer during bonding, enhances the stability of the product, and avoids the instability problems caused by the wet engraving process.
Smart Images

Figure CN119028735A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of capacitor production, and in particular to a ceramic capacitor with a MIM structure and a production method thereof. Background Art
[0002] At present, capacitors with MIM (metal / insulating layer / metal) structure have attracted more and more researchers' attention due to their simple structure and good stability, and have been applied in various fields. In the production process of this type of capacitor, the most common method is to sputter metal film layers on the upper and lower surfaces of the insulating layer with a high dielectric constant (such as ceramic, etc.). In this production process, due to the small size of the capacitor itself (a few hundred microns in size), the metal film layer is sputtered on a larger area of ceramic dielectric layer (centimeter range), and finally the upper and lower electrodes of the micron-level capacitor are formed by wet etching patterning process;
[0003] However, due to the isotropic etching characteristics of the etching solution, the wet etching process also has the characteristic of isotropic non-selectivity, resulting in lateral etching of the upper electrode of the produced capacitor. The width of the middle and bottom of the upper electrode becomes smaller, forming a cross-section that is approximately inverted trapezoidal, affecting the reliability of the product. Summary of the invention
[0004] In view of the above-mentioned defects or deficiencies in the prior art, it is desirable to provide a ceramic capacitor with a MIM structure and a production method thereof.
[0005] In a first aspect, an embodiment of the present application provides a ceramic capacitor with a MIM structure, comprising:
[0006] Dielectric layer,
[0007] A first metal layer, disposed at the bottom of the dielectric layer;
[0008] A plurality of second metal layers are arranged and distributed on the top of the dielectric layer along the first direction, and the cross-section shape of each of the second metal layers is a regular trapezoid.
[0009] According to the technical solution provided in the embodiment of the present application, each of the second metal layers has a first inclined surface on both sides along the first direction, and the angle between each of the first inclined surfaces and the top surface of the dielectric layer is 95-124°.
[0010] In a second aspect, an embodiment of the present application provides a method for producing a ceramic capacitor with a MIM structure, comprising the following steps:
[0011] S100. Preprocessing, obtaining a ceramic plate, preprocessing the ceramic plate to obtain the dielectric layer, wherein the normal direction of the dielectric layer is the second direction;
[0012] S200. Photoresist treatment, coating the top surface of the dielectric layer with photoresist and preliminarily treating it to form a template, the template comprising the dielectric layer and a plurality of raised modules arranged on the dielectric layer along the first direction, the second direction being perpendicular to the first direction;
[0013] S300. Processing the metal layer, sputtering a metal layer onto the top and bottom surfaces of the template to form an intermediate component, wherein the intermediate component includes the template component, the first metal layer disposed at the bottom of the dielectric layer, a plurality of second metal layers disposed at the top of the dielectric layer and between the protruding modules, and a plurality of third metal layers disposed at the top of each of the protruding modules;
[0014] S400. Finishing processing, removing each of the protruding modules and each of the third metal layers on the intermediate component to obtain the ceramic capacitor.
[0015] According to the technical solution provided in the embodiment of the present application, step S100 specifically includes the following steps:
[0016] S101. Obtaining a ceramic plate, wherein the ceramic plate is a preliminary blank after grinding and polishing;
[0017] S102. The ceramic plate is placed in deionized water for 5-10 minutes, and then placed in a cleaning solution for 5-10 minutes, and the cycle is repeated 3-5 times;
[0018] S103. The cleaned ceramic plate is placed in an oven at 120-150°C for drying;
[0019] S104. The dried ceramic plate is placed in a muffle furnace at 800-1000° C. and calcined for 3-5 hours, and then taken out and cooled to form the dielectric layer.
[0020] According to the technical solution provided in the embodiment of the present application, step S200 specifically includes the following steps:
[0021] S201. Coating a photoresist on the top surface of the dielectric layer to form the photoresist layer;
[0022] S202. The photoresist layer is pre-baked at a temperature of 90-120°C for a pre-baking time of 90-150 seconds;
[0023] S203. Dividing the photoresist layer into a molding area and a non-exposure area, wherein the molding area and the non-exposure area are alternately arranged along the first direction;
[0024] S204. Exposing the photoresist in the molding area to form the protruding module in the molding area;
[0025] S205. Remove the photoresist in the non-exposed area to form the template.
[0026] According to the technical solution provided in the embodiment of the present application, step S300 specifically includes the following steps:
[0027] S301. Sputtering the top surface of the template to form a primary sputtering member, the primary sputtering member comprising a dielectric layer, a plurality of second metal layers disposed on the top of the dielectric layer and between the protruding modules, and a plurality of third metal layers disposed on the top of each of the protruding modules;
[0028] S302. Sputtering a metal layer onto the bottom surface of the dielectric layer in the initial sputtering component to form the intermediate component.
[0029] According to the technical solution provided in the embodiment of the present application, the cross-section of the protruding module is an inverted trapezoid, and the angle between the side surface of the inverted trapezoid and the top surface of the dielectric layer is 56-85°.
[0030] According to the technical solution provided in the embodiment of the present application, step S400 specifically includes the following steps:
[0031] S411. Covering the top surface of the intermediate member with a UV film, wherein the bottom surface of the UV film is bonded to the top surface of the third metal layer;
[0032] S412. Peeling off the UV film, driving the third metal layer to separate from the top of the protruding module to form a semi-finished product;
[0033] S413. Soak the semi-finished product in a stripping solution for 2-5 minutes;
[0034] S414. Take out the semi-finished product after soaking, and remove the protruding modules on the semi-finished product to form the ceramic capacitor.
[0035] According to the technical solution provided in the embodiment of the present application, the step S411 further includes the following steps:
[0036] S410. Soak the intermediate piece in the stripping solution for 2-5 minutes.
[0037] According to the technical solution provided in the embodiment of the present application, step S400 specifically includes the following steps:
[0038] S420. Soaking the intermediate member in a stripping solution for 5-10 minutes;
[0039] S421. Take out the soaked middle piece, and remove the protruding modules on the middle piece to form the ceramic capacitor.
[0040] Compared with the prior art, the beneficial effects of the present invention are:
[0041] The present invention forms an electrode through a first metal layer and a second metal layer, and the second metal layer is formed into a regular trapezoidal cross-section. When the capacitor is produced, the top surface area of the upper electrode is limited, that is, the top surface area of the second metal layer is limited, and the bottom surface area of the regular trapezoid is larger, and the connection with the dielectric layer is more stable. In the subsequent bonding process of this structure, it is less likely for the gold wire to tear the edge of the second metal layer from the dielectric layer, and the product reliability is higher. In addition, by first coating a photoresist and then sputtering a metal layer, the photoresist and the excess metal layer are finally removed, and the second metal layer of the ceramic capacitor is finally used as the upper electrode of the capacitor. Compared with the wet etching process that uses an etching solution to erode the metal layer, the etching solution will laterally erode the upper electrode. In the present invention, the photoresist has formed a protruding module before the metal layer is sputtered, and the second metal layer is located between the protruding modules. The solution for removing the photoresist will not affect the second metal layer, which effectively solves the problem of product instability caused by the wet etching process.
[0042] It should be understood that the contents described in the summary of the invention are not intended to limit the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0044] Figure 1 A flowchart of a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0045] Figure 2 A schematic structural diagram of a first coating member in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0046] Figure 3 A schematic diagram of the structure of the non-exposure area and the forming area in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0047] Figure 4 A schematic diagram of the structure of a template member in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0048] Figure 5 A schematic diagram of the structure of a primary sputtering part in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0049] Figure 6 A schematic diagram of the structure of an intermediate component in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0050] Figure 7 A schematic structural diagram of a semi-finished product in a method for producing a ceramic capacitor with a MIM structure provided in an embodiment of the present application;
[0051] Figure 8 A schematic structural diagram of a ceramic capacitor with a MIM structure provided in an embodiment of the present application.
[0052] Numbers in the figure: 1, dielectric layer; 2, photoresist layer; 21, raised module; 22, non-exposed area; 23, molding area; 3, intermediate part; 31, first metal layer; 32, second metal layer; 33, third metal layer; 34, initial sputtering part; 4, template part; 41, first coating part; 5, ceramic capacitor; 51, semi-finished product. DETAILED DESCRIPTION
[0053] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should also be noted that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.
[0054] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0055] Example 1
[0056] Please refer to Figure 8 , an embodiment of the present invention provides a ceramic capacitor of a MIM structure, comprising:
[0057] Dielectric layer 1,
[0058] The first metal layer 31 is disposed at the bottom of the dielectric layer 1;
[0059] A plurality of second metal layers 32 are arranged and distributed on the top of the dielectric layer 1 along the first direction. The cross-sectional shape of each second metal layer 32 is a regular trapezoid. The first direction is Figure 8 In the left and right directions in the actual production process, the top surface area of the second metal layer 32 will be limited, while the bottom surface area of the second metal layer 32 is larger, and the connection with the dielectric layer 1 is more stable. In the subsequent bonding process, this structure makes it more difficult for the gold wire to tear the edge of the second metal layer 32 from the dielectric layer 1, and the product reliability is higher;
[0060] In some embodiments, each second metal layer 32 has a first inclined surface on both sides along the first direction, and the angle between each first inclined surface and the top surface of the dielectric layer 1 is 95-124°. Figure 8As shown, preferably, the angle is 115°, which ensures the bonding strength between the second metal layer 32 and the dielectric layer 1 after molding, and also prevents adjacent second metal layers 32 from being too close to each other and causing interference.
[0061] Example 2
[0062] Please refer to Figures 1 to 8 The embodiment of the present invention provides a method for producing a ceramic capacitor with a MIM structure, comprising the following steps:
[0063] S100. Preprocessing, obtaining a ceramic plate, preprocessing the ceramic plate, obtaining a dielectric layer 1, the normal direction of the dielectric layer 1 is a first direction, and the first direction is Figure 2 The vertical direction in
[0064] S101 obtains a ceramic plate, the ceramic plate is a preliminary blank after grinding and polishing; wherein, in this embodiment, the ceramic plate thickness of 150 microns is selected, by grinding and polishing, to ensure that the surface of the ceramic plate is smooth and flat, to facilitate subsequent coating of photoresist and sputtered metal layer;
[0065] S102. Wash the ceramic plate in deionized water for 5 minutes, then wash it in a cleaning solution for 5 minutes, and repeat this cycle 3 times; clean the debris and dust on the surface of the ceramic plate to avoid interference with subsequent processes;
[0066] S103. The cleaned ceramic plate is placed in an oven at 120°C for drying;
[0067] S104. The dried ceramic plate is placed in a muffle furnace at 800°C and calcined for 3 hours, and then taken out and cooled to form a dielectric layer 1;
[0068] Among them, by calcining the ceramic plate, the carbon-containing organic matter inside the ceramic plate is eliminated, and the surface roughness caused by the carbon-containing substances is reduced. At the same time, calcination can soften the surface of the ceramic plate, thereby repairing the microcracks on the surface of the ceramic plate caused by grinding, and repairing the depressions left after eliminating the carbon-containing substances, reducing microcracks and depressions, and improving the integrity of the dielectric layer 1.
[0069] S200. Photoresist treatment, coating the top surface of the dielectric layer 1 with photoresist and preliminarily treating it to form a template member 4, the template member 4 comprising a dielectric layer 1 and a plurality of raised modules 21 arranged on the dielectric layer 1 and distributed along a second direction, the second direction being perpendicular to the first direction;
[0070] S201. Coating a photoresist on the top surface of the dielectric layer 1 to form a photoresist layer 2;
[0071] Among them, Figure 2As shown, the photoresist is a negative photoresist. In this embodiment, the photoresist layer 2 is selected to have a thickness of 10 microns, and the RN218 series can be selected. Alternatively, the photoresist can also be selected from the RN246 series, Az nLOF 2000 series, and RPN-1150-90N1. In addition, further optionally, spin coating or spray coating is selected according to the thickness of the photoresist layer 2 and the viscosity of the photoresist solution. For example, if the thickness of the photoresist layer 2 is greater than 6 microns, spray coating is generally selected as the coating method. If the thickness of the photoresist layer 2 is less than 6 microns, spin coating is generally selected as the coating method. The spin coating speed is 500-3000rpm. Spin coating is more stable, and the spin coating speed is determined according to the actual thickness of the photoresist layer 2. The smaller the speed, the thicker the coating.
[0072] S202. The photoresist layer 2 is pre-baked at a temperature of 90°C for 90 seconds;
[0073] Among them, pre-baking refers to allowing the solvent in the photoresist layer 2 to escape slowly and fully at a corresponding ambient temperature, so that the photoresist layer 2 can be better adhered to the top of the dielectric layer 1;
[0074] S203. The photoresist layer 2 is divided into a molding region 23 and a non-exposure region 22, the molding region 23 and the non-exposure region 22 are staggered along the second direction, the molding region 23 and the non-exposure region 22 are as Figure 3 As shown;
[0075] S204. Exposing the photoresist in the molding area 23 to form a protruding module 21 in the molding area 23;
[0076] Among them, Figure 3 and Figure 4 As shown, exposure refers to the light emitted by the illumination light source being irradiated onto the mask through a converging lens, generating diffraction light beams through the mask, and these diffraction light beams carry the graphic information on the mask. The light beams are focused onto the surface of the photoresist layer 2 through a projection lens, and an image of the mask pattern is formed on the surface of the photoresist layer 2. In this step, the non-exposure area 22 is shielded to solidify the softened photoresist in the molding area 23.
[0077] S205. Remove the photoresist in the non-exposed area 22 to form a template member 4;
[0078] This step is also called development, which is to dissolve the unfixed photoresist, that is, the photoresist in the non-exposed area 22, by a chemical developer, so as to achieve the purpose of retaining the protruding module 21;
[0079] S300. Processing the metal layer, sputtering a metal layer onto the top and bottom surfaces of the template member 4 to form an intermediate member 3, wherein the intermediate member 3 includes the template member 4, a first metal layer 31 disposed at the bottom of the dielectric layer 1, a plurality of second metal layers 32 disposed at the top of the dielectric layer 1 and between the protruding modules 21, and a plurality of third metal layers 33 disposed at the top of each protruding module 21;
[0080] S301. The top surface of the template 4 is sputtered to form a primary sputtered member 34, the primary sputtered member 34 comprising a dielectric layer 1, and a plurality of second metal layers 32 disposed at the top of the dielectric layer 1 and between the protruding modules 21, and a plurality of third metal layers 33 disposed at the top of each protruding module 21. The primary sputtered member 34 is as follows. Figure 5 As shown;
[0081] S302. Sputtering a metal layer onto the bottom surface of the dielectric layer 1 in the initial sputtering member 34 to form an intermediate member 3, the intermediate member 3 is as follows Figure 6 As shown;
[0082] Among them, Figure 5 and Figure 6 As shown, the sputtering vacuum degree of the two metal layer sputterings is 0.5 Pa, and the sputtering power is 400-1000W to prevent the metal ions in the sputtering process from damaging the dielectric layer 1 or the photoresist layer 2. The sputtering time is determined according to the required thickness of the first metal layer 31 and the second metal layer 32. The longer the time, the thicker the metal layer.
[0083] S400. Finishing treatment, removing each protruding module 21 and each third metal layer 33 on the intermediate member 3, and obtaining a ceramic capacitor 5; the ceramic capacitor 5 is as follows Figure 8 shown.
[0084] In some embodiments, the thicknesses of the first metal layer 31, the second metal layer 32 and the third metal layer 33 are equal, and the thickness of the photoresist layer 2 is 1.5 to 3 times that of the first metal layer 31. According to the thickness of the photoresist being 10 microns, the thickness of the first metal layer 31 can be selected to be 3.5 microns. Figure 6 As shown, the thicker photoresist layer 2 can separate the third metal layer 33 and the second metal layer 32, thereby preventing the third metal layer 33 from being inconvenient to remove due to contact between the two.
[0085] In some embodiments, the cross section of the protrusion module 21 is an inverted trapezoid, and the angle between the side surface of the inverted trapezoid and the top surface of the dielectric layer 1 is 56-85°;
[0086] The top of the photoresist in the molding area 23 is more likely to receive energy, while the bottom is less likely to receive energy. The top is more completely cured, while the bottom is less likely to be completely cured. The user sets the exposure dose according to the specific thickness of the photoresist layer 2, so that the top is completely cured, and only the central area of the bottom is cured, and the bottom edge is still not softened. In this way, after development, the retained protruding module 21 will present an inverted trapezoidal shape with a larger cross section at the top and a smaller cross section at the bottom. The first inclined surfaces on the left and right sides of the second metal layer 32 formed in this way are at an angle of 95-124° to the top surface of the dielectric layer 1, because the top surface of the upper electrode will be aligned during capacitor production. The area of the second metal layer 32 is limited, that is, the area of the top surface of the second metal layer 32 is limited, while the bottom surface area of the right trapezoid of the second metal layer 32 is larger, and the connection with the dielectric layer 1 is more stable. In the subsequent bonding process, the gold wire of this structure is less likely to tear the edge of the second metal layer 32 off the dielectric layer 1, and the product reliability is higher. Preferably, the angle between the side surface of the inverted trapezoid and the top surface of the dielectric layer 1 is 65°, and the angle between the side surface of the formed second metal layer 32 and the bottom surface of the dielectric layer is 115°, which ensures the molding and strength of the second metal layer 32 without causing the adjacent second metal layers 32 to be too close.
[0087] Example 3
[0088] Based on Example 2, step S400 in this embodiment specifically includes the following steps:
[0089] S411. Cover the top surface of the middle piece 3 with a UV film, and the bottom surface of the UV film is bonded to the top surface of the third metal layer 33; wherein, optionally, the adhesion of the UV film is 20 Newtons per 25 mm, and the thickness is 100 microns, and it has good adhesion.
[0090] S412. Peeling off the UV film drives the third metal layer 22 to separate from the top of the protruding module 21 to form a semi-finished product 51. The semi-finished product 51 is as shown in FIG. Figure 7 As shown;
[0091] S413. Soak the semi-finished product 51 in a stripping solution for 2 minutes. The temperature of the stripping solution is 40°C. The stripping solution softens each protruding module 21 to reduce the adhesion between the protruding module 21 and the dielectric layer 1.
[0092] S414. Take out the semi-finished product 51 after soaking, and remove the protruding modules 21 on the semi-finished product 51 to form a ceramic capacitor 5 such as Figure 8 shown.
[0093] Example 4
[0094] Based on Example 2, step S400 in this embodiment specifically includes the following steps:
[0095] S410. Soak the intermediate member 3 in a stripping solution for 2 minutes. The temperature of the stripping solution is 40° C. to reduce the adhesion between the third metal layer 33 and the protruding module 21, so as to facilitate the subsequent removal of the third metal layer 33;
[0096] S411. Cover the top surface of the middle piece 3 with a UV film, and the bottom surface of the UV film is bonded to the top surface of the third metal layer 33; wherein, optionally, the adhesion of the UV film is 20 Newtons per 25 mm, and the thickness is 100 microns, and it has good adhesion.
[0097] S412. Peeling off the UV film drives the third metal layer 22 to separate from the top of the protruding module 21 to form a semi-finished product 51. The semi-finished product 51 is as shown in FIG. Figure 7 As shown;
[0098] S413. Soak the semi-finished product 51 in a stripping solution for 2 minutes. The temperature of the stripping solution is 40°C. The stripping solution softens each protruding module 21 to reduce the adhesion between the protruding module 21 and the dielectric layer 1.
[0099] S414. Take out the semi-finished product 51 after soaking, and remove the protruding modules 21 on the semi-finished product 51 to form a ceramic capacitor 5 such as Figure 8 shown.
[0100] Example 5
[0101] Based on Example 2, step S400 in this embodiment specifically includes the following steps:
[0102] S420. Soak the intermediate member 3 in a stripping solution for 10 minutes. The temperature of the stripping solution is 60° C. Through a long period of soaking, each protruding module 21 is softened, and the adhesion between the protruding module 21 and the dielectric layer 1 is fully reduced, so that the protruding module 21 and the corresponding third metal layer 33 can be directly removed together in the subsequent process;
[0103] S421. Take out the soaked middle piece 3 and remove the protruding modules 21 on the middle piece 3 to form a ceramic capacitor 5. Figure 8 shown.
[0104] In the description of this specification, the terms "connection", "installation", "fixation" and the like should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0105] In the description of this specification, the description of the terms "one embodiment", "some embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0106] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A ceramic capacitor with a MIM structure, characterized in that: include: Dielectric layer (1), A first metal layer (31) is disposed at the bottom of the dielectric layer (1); A plurality of second metal layers (32) are arranged and distributed on the top of the dielectric layer (1) along a first direction, and each second metal layer (32) has a cross-sectional shape of a regular trapezoid.
2. The ceramic capacitor of the MIM structure according to claim 1, characterized in that: Each of the second metal layers (32) has a first inclined surface on both sides along the first direction, and the angle between each of the first inclined surfaces and the top surface of the dielectric layer (1) is 95-124°.
3. The method for producing a ceramic capacitor with a MIM structure according to claim 2, characterized in that: The steps include: S100. Preprocessing, obtaining a ceramic plate, preprocessing the ceramic plate to obtain the dielectric layer (1), wherein the normal direction of the dielectric layer (1) is the second direction; S200. Photoresist treatment, coating the top surface of the dielectric layer (1) with photoresist and preliminarily treating it to form a template (4), wherein the template (4) comprises the dielectric layer (1) and a plurality of protruding modules (21) arranged on the dielectric layer (1) and distributed along the first direction, wherein the second direction is perpendicular to the first direction; S300. Processing the metal layer, sputtering a metal layer onto the top and bottom surfaces of the template member (4) to form an intermediate member (3), wherein the intermediate member (3) comprises the template member (4), the first metal layer (31) disposed at the bottom end of the dielectric layer (1), a plurality of second metal layers (32) disposed at the top end of the dielectric layer (1) and located between the protruding modules (21), and a plurality of third metal layers (33) disposed at the top end of each of the protruding modules (21); S400. Finishing processing, removing each of the protruding modules (21) and each of the third metal layers (33) on the intermediate component (3) to obtain the ceramic capacitor (5).
4. The method for producing a ceramic capacitor with a MIM structure according to claim 3, characterized in that: The step S100 specifically includes the following steps: S101. Obtaining a ceramic plate, wherein the ceramic plate is a preliminary blank after grinding and polishing; S102. The ceramic plate is placed in deionized water for 5-10 minutes, and then placed in a cleaning solution for 5-10 minutes, and the cycle is repeated 3-5 times; S103. The cleaned ceramic plate is placed in an oven at 120-150°C for drying; S104. The dried ceramic plate is placed in a muffle furnace at 800-1000° C. and calcined for 3-5 hours. The ceramic plate is taken out and cooled to form the dielectric layer (1).
5. The method for producing a ceramic capacitor with a MIM structure according to claim 3, characterized in that: The step S200 specifically includes the following steps: S201. Coating a photoresist on the top surface of the dielectric layer (1) to form the photoresist layer (2); S202. The photoresist layer (2) is pre-baked at a temperature of 90-120°C and a pre-baking time of 90-150 seconds; S203. Dividing the photoresist layer (2) into a forming area (23) and a non-exposure area (22), wherein the forming area (23) and the non-exposure area (22) are arranged alternately along the first direction; S204. Exposing the photoresist in the molding area (23), so that the molding area (23) forms the protruding module (21); S205. Remove the photoresist in the non-exposed area (22) to form the template (4).
6. The method for producing a ceramic capacitor with a MIM structure according to claim 5, characterized in that: The step S300 specifically includes the following steps: S301. Sputtering the top surface of the template member (4) to form a primary sputtering member (34), wherein the primary sputtering member (34) comprises a dielectric layer (1), a plurality of second metal layers (32) disposed on the top of the dielectric layer (1) and between the protruding modules (21), and a plurality of third metal layers (33) disposed on the top of each of the protruding modules (21); S302. Sputtering a metal layer onto the bottom surface of the dielectric layer (1) in the initial sputtering component (34) to form the intermediate component (3).
7. The method for producing a ceramic capacitor with a MIM structure according to claim 6, characterized in that: The cross section of the protruding module (21) is an inverted trapezoid, and the angle between the side surface of the inverted trapezoid and the top surface of the dielectric layer (1) is 56-85°.
8. The method for producing a ceramic capacitor with a MIM structure according to claim 7, characterized in that: The step S400 specifically includes the following steps: S411. Covering the top surface of the intermediate member (3) with a UV film, wherein the bottom surface of the UV film is bonded to the top surface of the third metal layer (33); S412. Peeling off the UV film, driving the third metal layer (22) to separate from the top of the protruding module (21), to form a semi-finished product (51); S413. The semi-finished product (51) is placed in a stripping solution and soaked for 2-5 minutes; S414. Take out the semi-finished product (51) after soaking, and remove the protruding modules (21) on the semi-finished product (51) to form the ceramic capacitor (5).
9. The method for producing a ceramic capacitor with a MIM structure according to claim 8, characterized in that: The step S411 also includes the following steps: S410. Soak the intermediate component (3) in the stripping liquid for 2-5 minutes.
10. The method for producing a ceramic capacitor with a MIM structure according to claim 7, characterized in that: The step S400 specifically includes the following steps: S420. Soak the intermediate member (3) in a stripping solution for 5-10 minutes; S421. Take out the soaked intermediate piece (3), and remove the protruding modules (21) on the intermediate piece (3) to form the ceramic capacitor (5).
Citation Information
Cited By
Laser conducting layer structure, preparation method thereof and laser
CN120601242A