Glue for plates
Through the Maillard reaction gum and hyperbranched polyamide based on amines and carbohydrates, the problems of formaldehyde emission and insufficient reactivity of traditional gums are solved, and the production of cellulose-containing plates with high performance and low environmental impact are achieved.
Patent Information
- Application Number
- CN202380037327.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-25
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-26
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to a board comprising cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, and a curing glue for bonding these cellulose-containing materials together. The present invention also relates to a method for making such a board, a glue for said board and a method for preparing said glue.
[0002] The present invention relates to boards containing cellulose-containing materials. These cellulose-containing materials may include one or more of the following materials: wood fibers, wood chips, wood flakes, wood layers, flax fibers, bamboo fibers, hemp fibers, wood wastes derived from, for example, particleboards / wood fiberboards, etc., etc. Therefore, these cellulose-containing materials may be, for example, wood-containing cellulose materials. These boards are, for example, wood fiberboards, such as MDF (medium density fiberboard) and HDF (high density fiberboard), other wood-based panels such as particleboards, OSB (oriented strand board), composite panels (multiplex board), etc., and non-wood-based fiberboards such as flax boards, bamboo boards, hemp boards, etc. These boards may or may not be partially or completely made of recycled materials (such as recycled wood-containing cellulose materials). Therefore, the cellulose-containing material may include recycled materials derived from recycling, for example, particleboards, wood fiberboards, or panels containing such particleboards or wood fiberboards. Therefore, particleboards may include particles of recycled particleboards, or wood fiberboards may include particles of recycled wood fiberboards, such as recycled wood fibers. Background Art
[0003] The most common glues used in the production of said boards are aminoplast polymers, which are prepared by polycondensation of urea and formaldehyde to form urea-formaldehyde resins (UF resins). Optionally, melamine is added and melamine-urea-formaldehyde resins (MUF resins) are obtained, or melamine and phenol (MUPF resins: melamine-urea-phenol-formaldehyde resins). The great advantages of these glues are their low cost, since in their preparation generally available and inexpensive raw materials are used; and their high reactivity. Such glues may release formaldehyde during and after the polymerization, under the influence of changes in temperature, humidity or pH. There is an increasing search to limit the formaldehyde emission of the boards or even to reduce it to zero. Therefore, there is a constant search for formaldehyde-free glues for the production of said boards.
[0004] US 2006 / 0163769 describes the use of water glass glue for producing fire-resistant derived wood products.
[0005] A known formaldehyde-free glue used to produce derived wood products consists of the polymer methylene diphenyl diisocyanate (pMDI).
[0006] CA2019382A1 describes a mixture of an isocyanate and a sufficient amount of a metal soap for use as a glue in a derived wood product. The metal soap is used as a blocking compound to prevent the reaction between water and the isocyanate, so a sufficient amount of the metal soap is required. CA2019382A1 further describes that for the mixture of the isocyanate and a sufficient amount of the metal soap, water glass may also be included in the mixture to form an emulsion.
[0007] A further disadvantage of all of the above-mentioned glues is that they are based on fossil raw materials.
[0008] Bio-based glues for boards are already available, but the production of boards with the help of these glues is not so simple. Disadvantages include too low reactivity, uncontrolled / unsatisfactory prepolymerization, limited adhesion, poor wetting compared to common formaldehyde-containing aminoplast glues. Examples of bio-based glues are glues based on lignin, plant flours (such as soy flour) or sugars. Summary of the invention
[0009] The present invention relates to a glue based on amines and carbohydrates, the cured glue therefore present in the board comprising Maillard reaction products derived from the Maillard reaction between these amines and carbohydrates. Firstly, the object of the present invention is to optimize this glue and the board comprising this glue.
[0010] According to a first aspect, the invention relates to a board comprising cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, and a cured glue for bonding these cellulose-containing materials together, wherein the cured glue is derived from a glue based on amines and carbohydrates, and the cured glue comprises a Maillard reaction product derived from a Maillard reaction between these amines and carbohydrates, wherein the glue further comprises an additive for controlling the Maillard reaction. To form such a board, a glue based on amines and carbohydrates and comprising additives is used, wherein this glue has not yet been cured or has not yet been completely cured. During the formation of the board, this glue will (further) cure, thereby forming a cured glue that bonds the cellulose-containing materials together. Here, "cured glue" means a glue that has already cured during the board forming process, which is dry enough and fully bonds the cellulose-containing materials together, so as to produce the desired board. This does not in itself mean that the glue is completely cured. Here, the cured glue may or may not be a completely cured glue. For the boards, such as fiberboards, particleboards, OSB boards, composite boards, etc., heat is generated and / or added during the production process, for example during the pressing of these boards. By heating, the Maillard reaction is initiated, which may lead to further curing of the glue used. Here, "cured glue derived from amine and carbohydrate based glue" refers to the glue produced after the glue used to form the board is cured.
[0011] The glue used to form such a board is based on the amines, carbohydrates and additives. This means that these amines, carbohydrates and additives will be provided during the glue formation process. The percentages, amounts, proportions of these amines, carbohydrates and additives are always expressed here based on the amount of dry matter provided for the glue formation. This is because during the glue formation process, before the glue is used to form the board, these amines and carbohydrates have (partially) reacted with each other. The amount of cellulose-containing material is preferably expressed as the dry matter of the cellulose-containing material (thus dry cellulose-containing material, such as dry wood).
[0012] By means of additives, it is preferred that the Maillard reaction is closely controlled during the formation of the board, so as to form the desired Maillard reaction product and / or obtain the desired reaction rate, thereby optimizing the performance of the cured glue and the performance of the formed board. Therefore, the additive can increase the reactivity of the glue and / or offset the undesirable prepolymerization and / or increase the adhesion of the cured glue. The result is a board with the desired tensile strength, bending strength, E-modulus, etc. Therefore, the additive provides a better glue. With this glue, we can choose to make a board with better performance compared to the board made using the existing glue based on carbohydrates and amines. However, we can also choose to use less glue than the board made using the existing glue based on carbohydrates and amines to obtain similar performance. By means of the above-mentioned additives, we can also choose to reduce the content of amines in the glue. Good results are obtained when the weight percentage of amines in the total weight of amines and carbohydrates is at least 20. For example, we can then choose to use less amines, thereby selecting the weight percentage of amines in the total weight of amines and carbohydrates to be at most 20 or at most 15, to obtain performance similar to boards such as those made using the existing glue based on carbohydrates and amines.
[0013] The Maillard reaction is a general term for a series of complex chemical reactions that occur between reducing sugars and amines. Carbohydrates and amines form Maillard reactants here. The above additives may or may not be used for the Maillard reaction and may or may not form part of the Maillard reactants. One or more types of additives may be used.
[0014] Amines are compounds containing at least one amine radical and are therefore a source of amines. The sum of the dry matter of amines used to form the glue and the dry matter of carbohydrates in the dry matter of the cellulose-containing material is, for example, 2 to 20, preferably 3 to 15, even more preferably 4 to 10 weight percentages. We are talking here about the dry matter of amines used to form the glue and the dry matter of carbohydrates, because during the formation of the glue, i.e. during the mixing of the components of the glue, these components may have reacted with each other, wherein, for example, water is formed, so that the dry matter content changes. The above amounts are also determined by the type of board, for example, for a three-layer particleboard comprising a central layer and two outer covering layers, the weight percentage is, for example, 3% to 12% in all layers, wherein the weight percentage of the covering layers is always higher than the weight percentage of the central layer. Thus, for the covering layers, the weight percentage can be, for example, 6, 7, 8, 9, 10, 11 or 12. For the central layer, the weight percentage can be, for example, 3, 4, 5, 6, 7 or 8. For MDF or HDF or OSB, the weight percentage can be 5 to 10, thus, for example, 6, 7, 8 or 9.
[0015] The amine, for example, accounts for 15 wt% to 40 wt%, preferably 20 wt% to 30 wt%, or preferably 35 wt% to 40 wt% of the total weight of the amine and the carbohydrate. Then, the carbohydrate accounts for 60 wt% to 85 wt%, preferably 70 wt% to 80 wt%, or preferably 60 wt% to 65 wt% of the total weight of the amine and the carbohydrate. The amine may, for example, include a diamine such as hexamethylenediamine (HDMA), or an amide containing an amine group, or a hyperbranched polyamide. Thus, the weight percentage of the amine in the total weight of the amine and the carbohydrate may be, for example, 22, 23, 24, 25, 26, 27, 28, 35, 36, 37 or 38.
[0016] The carbohydrate is a reducing sugar and / or is converted into a reducing sugar. Reducing sugars are necessary for the Maillard reaction. Therefore, sucrose can be used, for example, converted into glucose and fructose. Sucrose is a widely available sugar and a cheap bio-based carbohydrate source. It can start with a 50 wt% to 70 wt% aqueous solution of sucrose. It can also start with invert sugar. The carbohydrate used can also contain only glucose or only fructose. A 65 wt% to 75 wt% aqueous solution of invert sugar, for example a 70 wt% aqueous solution of invert sugar, can be used. The solution is then contacted with an amine.
[0017] "Carbohydrate and amine based gum" refers to a gum whose dry matter consists mainly of carbohydrates and amines, e.g. at least 50 wt% carbohydrates and amines, preferably at least 70 wt%, and even more preferably at least 80 wt%, and most preferably at least 90 wt% of the total weight of the dry matter. Preferably, the additives represent at most 20 wt%, preferably at most 10 wt%, and most preferably at most 5 wt% of the total weight of the dry matter.
[0018] During the manufacture of the glue for forming the board, the various components of the glue are combined. This glue is then used to bond the cellulose-containing material of the board, thereby forming the board. The above-mentioned board is usually formed by pressing, wherein heat is generated and / or added during the pressing process. The Maillard reaction occurs through this heat. The Maillard reaction may have partially occurred before pressing, that is, during the formation of the glue, and the glue already contains Maillard reaction products during the bonding of the cellulose-containing material. Therefore, during the combination of the components of the glue, heat may have been added, so that the Maillard reaction occurs. This has the advantage that during the bonding process, the glue already contains some Maillard reaction products, so the pressing time may be shortened and / or the reactivity of the glue is higher. Therefore, for example, we can proceed as follows: First, a pre-reactant containing a carbohydrate and a certain proportion of amine is prepared. The pre-reactant is heated (and / or the carbohydrate and / or the said proportion of amine are heated before being combined to form the pre-reactant). In this way, the Maillard reaction occurs during the formation of the pre-reactant, and the pre-reactant already has many Maillard reaction products. The remaining amine is then added to form a glue, which is then used to glue the cellulose-containing material. The pre-reactant may have included multiple additives or all additives. These additives can be added when the pre-reactant forms the beginning, or can be added during the pre-reactant formation and after the pre-reactant forms. The addition time of the additive may also depend on the type of the additive. In order to form the pre-reactant, for example, 5 wt% to 40 wt% of the amine can be provided, for example 15 wt% to 40 wt%, for example 20 wt% to 30 wt%, for example 10 wt% to 20 wt%, such as 10wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt% or 18 wt%, in this way, it is ensured that in the glue formed, there are still enough amines that have not yet reacted. If the additive comprises an acid or an acid salt, for example a salt of chloric acid (such as HCl) or hypochlorous acid (such as NaOCl), and the carbohydrate comprises sucrose, then preferably this acid or these acid salts are added to the pre-reactant so that sucrose is satisfactorily converted into glucose and fructose.
[0019] These cellulose-containing materials are preferably lignocellulose-containing materials. Plant fibers are, for example, wood fibers. These wood fibers may or may not be present in the form of wood fiber bundles.
[0020] Preferably, only one first type of glue is used to form the board, i.e. a glue based on the carbohydrate and amine, but the board may also include other types of glue. Thus, a glue mixture comprising the first type of glue and one or more other types of glue may be used, and / or the board may be multilayered, wherein the first type of glue is used for one of the layers and another type of glue is used for another layer. Examples of other glues are, for example, conventional UF glues, MUF glues, MUPF glues, pMDI glues, polyurethane glues, polyvinyl butyral glues, polyacrylate glues, etc. For example, polyurethane glues can be used to improve water resistance and / or flexibility. The board may also be formed with various glues of the first type of glue. Thus, the board may be multilayered, wherein different glues, but for example all glues based on the carbohydrate and amine, are used for different layers. These last mentioned various glues may be different on all kinds of surfaces. There is now a non-exhaustive list of possible differences, which can be combined with each other as long as they are not incompatible: dry matter content, additives (type and amount), carbohydrates (type and amount), amines (type and amount), solvents used (water or solvent), etc.
[0021] Preferably, the additive comprises a base. The pH value during the Maillard reaction is controlled by the base, so that the desired Maillard reaction product is formed. Surprisingly, it was found that potassium carbonate (K2CO3) is a base that is very suitable for use as an additive. K2CO3 is a base that can ensure a faster start of the Maillard reaction, but does not lead to undesirable prepolymerization of the glue. Preferably, the base also contains K2CO3, and even more preferably, the base only contains K2CO3. Prepolymerization refers to the polymerization of the glue before the forming (e.g. pressing) of the board, for example. The addition of K2CO3 does not lead to an undesirable increase in the viscosity of the glue. Other bases can also be used, such as the strong bases NaOH and KOH. The base can also contain Na2CO3 and / or Na2HPO4, and for example only one of these bases. NaOH and KOH may lead to undesirable prepolymerization, resulting in reduced technical properties of the board, so these are not very suitable. Two or more different bases can also be used. When a pre-reactant as described above is used, the pre-reactant preferably does not contain the base.
[0022] More preferably, the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the cured glue, wherein preferably, for this layer, the weight percentage of alkali to the cellulose-containing material is 0.03 to 1, preferably 0.1 to 1, preferably 0.4 to 1, even more preferably 0.15 to 0.25. Thus, the weight percentage of K2CO3 relative to the cellulose-containing material may be 0.1 to 1, preferably 0.15 to 0.25. The weight percentage here refers to the amount of dry matter of alkali, such as K2CO3, added during the glue formation process in the dry matter content of the cellulose-containing material used to form the board. The weight percentage of K2CO3 relative to the cellulose-containing material may be, for example, 0.05 to 0.1, such as 0.07 or 0.08. These values are very suitable for MDF, but can also be used for other boards. The weight percentage of K2CO3 relative to the cellulose-containing material may be, for example, 0.2 to 0.3, such as 0.21, 0.22, 0.25 or 0.26. These values are very suitable for particleboard, but can also be used for other boards.
[0023] Also more preferably, the ratio of K2CO3 to the total dry weight of the amine and the carbohydrate is 0.01 to 0.2, preferably 0.02 to 0.1, for example 0.04. The ratio may also be lower and may be 0.005 to 0.01, for example 0.08. The ratio is related to the ingredients used in the gel formation process. To form the gel, K2CO3 is preferably prepared as an aqueous solution of, for example, at least 40 wt% K2CO3 to facilitate addition and good mixing. Thus, an aqueous solution with 50 wt% K2CO3 or 60 wt% K2CO3 may be used to form the gel.
[0024] In a preferred embodiment, the additive comprises a salt of chloric acid, for example a salt of hypochlorous acid. The additive may also comprise chloric acid itself, such as HCl. Salts of hypochlorous acid promote the formation of Strecker degradation products during the Maillard reaction, so that a board with greater stiffness and / or less glue at the same stiffness can be obtained. Surprisingly, it has been found that sodium hypochlorite (NaOCl) has a particularly positive effect. Therefore, the salt of hypochlorous acid preferably comprises NaOCl, and even more preferably NaOCl. Other examples of possible salts of hypochlorous acid are potassium hypochlorite and calcium hypochlorite. Two or more different said salts may also be used.
[0025] More preferably, the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the curing glue, wherein preferably, for this layer, the weight percentage of the salt of chloric acid (or chloric acid itself) to the cellulose-containing material is 0.01 to 1, such as 0.1 to 1, such as 0.02 to 0.2 or 0.1 to 0.2. Possible weight percentages are 0.01, or 0.02, or 0.03. The weight percentage of NaOCl to the cellulose-containing material can be 0.1 to 1, preferably 0.1 to 0.2. The weight percentage here refers to the dry matter amount of the salt of hypochlorous acid, such as the amount of NaOCl, added during the glue formation process, based on the dry matter content of the cellulose-containing material used to form the board. If a pre-reactant is used for operation, for example, these salts of chloric acid (or chloric acid itself) constitute part of the pre-reactant.
[0026] Likewise, more preferably, the ratio of NaOCl to the total dry weight of the amine and carbohydrate is from 0.01 to 0.2, preferably from 0.02 to 0.1. The ratio of HCl to the total weight of the amine and carbohydrate is, for example, from 0.001 to 0.003. These ratios are related to the ingredients used in the glue formation process. To form the glue, it is preferred to use an aqueous solution of NaOCl, for example at least 40 wt% NaOCl, to facilitate addition and good mixing. Thus, an aqueous solution with 50 wt% NaOCl or 60 wt% NaOCl can be used to form the glue.
[0027] In a more preferred embodiment, the additive comprises a cross-linking agent, and these cross-linking agents preferably include intermediates produced during the Maillard reaction between the amine and the carbohydrate. In order to form the glue, the amine, the carbohydrate and the additional cross-linking agent that have not yet reacted with the reducing sugar will be provided. Through these cross-linking agents, the reactivity and therefore the quality of the glue are improved. The cross-linking agent preferably comprises at least one aldehyde group and at least one carboxyl group, followed by both aldehyde and carboxylic acid. When the cross-linking agent is used for the Maillard reaction, these cross-linking agents are regarded as Maillard reactants. In addition, by actively adding the intermediate, it is not necessary to wait until these intermediates are formed during the Maillard reaction, and it can be ensured that the various reaction pathways of the Maillard reaction are directly present at the beginning.
[0028] More preferably, the crosslinking agent is selected from the group comprising α-hydroxyaldehydes, glyceraldehydes and α-dicarbonyl compounds. The best results are obtained with α-dicarbonyl compounds, since they have the most positive influence on the reactivity of the gum. These α-dicarbonyl compounds may be, for example, dialdehydes and / or glyoxal and / or methylglyoxal and / or deoxyosone. α-Dicarbonyl compounds react with the amines present to form AGE products (advanced glycation end products), which can be classified as melanoidins if the molecular weight is above 10 kilodaltons.
[0029] When the cross-linking agents are intermediates formed in the Maillard reaction between the amine and the carbohydrate, these intermediates may have an impact on the viscosity of the glue used to form the board. Therefore, preferably, this is taken into account during the formation of the glue, i.e. during the mixing of the various ingredients. Therefore, it can be chosen when to add these cross-linking agents and / or how to mix. Therefore, these cross-linking agents can be added during the formation of the above-mentioned pre-reactant. These cross-linking agents can also be added after the pre-reactant is formed, but before the remaining amine is added to the pre-reactant. These cross-linking agents can even be added last, so after the remaining amine is added to the pre-reactant. Preferably, the cross-linking agents are added before the remaining amine is added. The cross-linking agents can also be added separately to the cellulose-containing material.
[0030] More preferably, the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the cured glue, wherein preferably, in the layer, the weight percentage of the cross-linking agent relative to the cellulose-containing material is 0.02 to 0.16, preferably 0.04 to 0.08. Here, the weight percentage refers to the amount of dry matter of the cross-linking agent, such as the amount of α-dicarbonyl compound, i.e., the amount of dialdehyde and / or glyoxal and / or methylglyoxal and / or deoxy-ketoose, which is added during the glue formation process, relative to the dry matter content of the cellulose-containing material.
[0031] Still more preferably, the ratio of α-dicarbonyl compounds, such as dialdehydes and / or glyoxal and / or methylglyoxal and / or deoxy-ketosugars to the total dry weight of amines and carbohydrates is 0.01 to 0.20, preferably 0.02 to 0.1. This ratio is related to the ingredients used in the glue formation process. In order to form the glue, glyoxal or another α-dicarbonyl compound is preferably prepared as an aqueous solution of, for example, at least 30 wt% glyoxal (or another α-dicarbonyl compound) to facilitate addition and good mixing. Therefore, an aqueous solution containing 40 wt% glyoxal or 50 wt% glyoxal can be used to form the glue.
[0032] In a specific embodiment, the additive comprises a metal-containing component, such as a metal oxide and / or a metal hydroxide and / or a metal salt forming a chelate. With the help of these metal-containing components, polymerization is enhanced and / or accelerated under the action of heat, thereby forming a very strong board. The weight percentage of the metal-containing component relative to the cellulose-containing material is, for example, 0.01 to 0.2, preferably 0.025 to 0.1. In addition, the addition of Ca(OH)2, Mg(OH)2 or CaCl2 can solidify the polymer formed after pressing the board, which contributes to the rigidity and strength of the board.
[0033] In a preferred embodiment, the additive comprises an amine crosslinking agent, wherein preferably these amine crosslinking agents are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes. When a pre-reactant as described above is used, the pre-reactant may or may not contain the amine crosslinking agent. For example, the pre-reactant may comprise an epoxide.
[0034] More preferably, the board comprises one or more layers, wherein at least one of said layers comprises said cellulose-containing material and said curing glue, wherein preferably for this layer the weight percentage of said amine cross-linking agent to cellulose-containing material is 0.05 to 0.25, such as 0.07 to 0.19. For MDF (or other boards), possible weight percentages are for example 0.17 or 0.18. For particleboard (or other boards), possible weight percentages are for example 0.07 to 0.12.
[0035] A second aspect of the invention is a board (optionally as defined in one or more embodiments of the first aspect indicated above) comprising a cellulose-containing material (such as plant fibers and / or wood chips and / or wooden parts), and a cured glue for bonding these cellulose-containing materials together, wherein the cured glue is derived from a glue based on amines and carbohydrates, and the glue comprises a Maillard reaction product derived from a Maillard reaction between these amines and carbohydrates, wherein at least a certain proportion of the amines is selected from the group comprising hyperbranched polyamides or chain amines; and wherein preferably at least a certain proportion of the amines are hyperbranched polyamides. The chain amine may, for example, comprise triethylenetetramine (TETA).
[0036] In the case of boards of the prior art, only HDMA is usually used as a source of amine. Using HDMA, boards of a certain quality can be manufactured. However, the production of HDMA has a high carbon footprint, since fossil raw materials are required for the industrial manufacture of HDMA. In addition, HDMA is corrosive. TETA is a good alternative to HDMA, but the production of TETA is usually carried out using fossil raw materials.
[0037] Surprisingly, it has been found that for glues based on amines and carbohydrates, hyperbranched polyamides can be used as amine sources. Thus, at least a certain proportion of the amines, and preferably at least 50% of the amines, even more preferably at least 70 wt% of the amines, and most preferably at least 90 wt% of the amines are hyperbranched polyamides. The remaining amines are then, for example, HDMA or TETA or a combination of HDMA and TETA. It can also be that all amines are hyperbranched polyamides. Surprisingly, this glue has particularly good adhesion. In addition, the process of producing boards with the aid of this glue can be carried out similarly to the production of the boards with conventional urea-formaldehyde glues (UF glues). Therefore,
[0038] Glues based on carbohydrates and amines (including hyperbranched polyamides) can also be used instead without causing major changes to the production process. These boards are obtained, for example, by providing glue to a cellulose-containing material and then pressing the cellulose-containing material provided with glue into a sheet material, wherein the sheet material is, for example, sawn into boards or has been formed into boards of the desired size. The pressing is preferably carried out at elevated temperatures, wherein the temperature can be up to more than 200°C.
[0039] Even more surprisingly, it has been found that boards comprising cellulose-containing materials that have been bonded together with a glue based on carbohydrates and amines (comprising hyperbranched polyamides) can show better technical properties than such boards comprising such glues (where the amines comprise only HDMA). Thus, higher stiffnesses (N / mm 2 ) and transverse tensile strength (N / mm 2 ) and / or higher water resistance.
[0040] Highly branched polyamides (hyperbranched polyamides) are highly branched three-dimensional macromolecules. High / strong branching means that the polyamide is not linear and also means that there is a large amount of branching. This means that there are more than 3, preferably more than 5, and even more preferably more than 10 branches in the polyamide macromolecule. The polyamide can be bio-based. Hyperbranched polyamides can be based on polycondensed amino acids, for example, wherein these amino acids are produced, for example, with the help of bacteria. In order to form these hyperbranched polyamides, groups or positions that do not block or hardly block amino acids can be selected. Therefore, the α position and / or ε position of the amino acid can be selected not to block. Bacteria such as Corynebacterium (Gram-positive) or Escherichia coli (Gram-negative) can chemically transform amino acids in a directed manner by fermentation, for example, mainly into lysine and a certain proportion of glutamine. Since in this case, the amines in the glue include hyperbranched polyamides, and the glue is also mainly composed of sugars, this glue also contributes to the sustainability of the board. In addition, this glue does not need to contain any formaldehyde, and preferably this glue does not contain any formaldehyde, so this glue also does not have the problem of possible formaldehyde release. When the hyperbranched polyamides are based on condensed amino acids, these are not necessarily based on only one type of amino acid. When using, for example, bacteria which form mainly lysine and small amounts of other amino acids such as glutamine, both lysine and glutamine can be used to produce the hyperbranched polyamides, so that an additional purification step of the amino acids is superfluous and the production of the hyperbranched polyamides can be carried out in an ecological manner.
[0041] Preferably, only one first type of glue is used to form the board, i.e., a glue based on the carbohydrate and amine, but the board may also include other types of glue. Therefore, a glue mixture comprising the first type of glue and one or more other types of glue may be used, and / or the board may be multilayered, wherein the first type of glue is used for one of the layers, and another type of glue is used for another layer. Examples of other glues are, for example, conventional UF glue, MUF glue, MUPF glue, pMDI glue, polyurethane glue, polyvinyl butyral glue, polyacrylate glue, etc. For example, polyurethane glue can be used to improve water resistance and / or flexibility. Boards may also be formed with various glues of the first type of glue. Therefore, the board may be multilayered, wherein various glues, but for example, all glues based on carbohydrates and amines, are used for various layers. These last mentioned various glues may be different on all kinds of surfaces. A non-exhaustive list of possible differences is given below, wherein as long as these differences are not contradictory, they can be combined with each other: dry matter content, amount of hyperbranched polyamide, average molecular weight (preferably number average molecular weight) of hyperbranched polyamide, amine (type and quantity), carbohydrate (type and quantity), additive (type and quantity), solvent (water or solvent).
[0042] In a preferred embodiment, the hyperbranched polyamide is obtained by polycondensation of amino acids, wherein these amino acids are preferably selected from the group containing arginine, glutamine, asparagine and lysine. Here, hyperbranched polyamides are obtained by peptide bonds, wherein, for example, the functional groups of amino acids are not preferred. Preferably, no position is blocked on the amino acids during the polycondensation process. Therefore, a complex polyamide network is obtained, which can well serve as an amine for the Maillard reaction. For example, hyperbranched polyamides are mainly obtained by polycondensation of lysine. Then the hyperbranched polyamide is, for example, a hyperbranched amino acid containing more than 80 wt%, preferably more than 90 wt% of lysine. Lysine is a basic amino acid that is cationic in a neutral medium. Lysine is obtained, for example, by fermentation using bacteria such as Corynebacterium or Escherichia coli. In the production process of lysine, other amino acids such as glutamine may also be formed in smaller amounts. By selecting bacteria, nutrients and fermentation conditions, the desired amino acids can be formed in a directed manner. For this fermentation, several carbohydrate sources can be used, such as sucrose, glucose, cellulose, hemicellulose, starch or lignin. As the ammonium source for fermentation, a mixture of ammonium salts, such as ammonium sulfate or diammonium phosphate, is generally used. Ammonium sulfate can be obtained as a byproduct in feces processing or after stripping ammonia-containing gas. In other words, the production of amino acids such as lysine may be carried out completely or mainly based on bio-based raw materials and / or waste. The hyperbranched polyamide obtained by amino acid polycondensation can be obtained by polycondensation from one, two, three or all four kinds of amino acids described in the group comprising arginine, glutamine, asparagine and lysine. Hyperbranched polyamide may also be obtained by polycondensation of amino acids selected from the group comprising arginine, glutamine, asparagine and lysine and one or more other amino acids.
[0043] In a specific embodiment, the hyperbranched polyamide comprises a first group of hyperbranched polyamides having an average molecular weight of 500 g / mol to 100000 g / mol, preferably 5000 g / mol to 50000 g / mol, and even more preferably 10000 g / mol to 25000 g / mol, wherein the first group of hyperbranched polyamides preferably accounts for at least 60 wt %, even more preferably at least 65 wt %, even more preferably at least 70 wt %, even more preferably at least 75 wt %, and most preferably at least 80 wt % of the hyperbranched polyamide. If the average molecular weight is higher than 5000 g / mol, the reactivity of the hyperbranched polyamide is optimal, and when the average molecular weight is lower than 50000 g / mol, gluing can be performed well. This can also allow good production of boards. The average molecular weight of the hyperbranched polyamide can be determined, for example, by low-angle laser light scattering (LALLS). As an alternative or in addition, the average molecular weight can be determined by gel permeation chromatography (GPC). Preferably, in this specification, the average molecular weight refers to the number average molecular weight.
[0044] In a preferred embodiment, the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the glue, wherein preferably in this layer the weight percentage of the hyperbranched polyamide relative to the cellulose-containing material is 0.5 to 4, preferably 0.5 to 3, for example 1 to 2. Possible weight percentages for MDF (or other boards) are, for example, 3 to 3.5. Possible weight percentages for particleboard (or other boards) are, for example, 1.8 to 2.2. At these weight percentages, the cellulose-containing material is preferably a dry cellulose-containing material, such as dry wood without any residual moisture. The weight ratio is preferably a weight ratio based on the weight of dry matter. Here, only 1 layer or only a plurality of layers may comprise the cellulose-containing material and the glue, while the other layers comprise, for example, another glue. Preferably, all of the layers comprise the cellulose-containing material and the glue based on carbohydrates and amines.
[0045] In a specific embodiment, the board comprises three or more layers, i.e. two outer covering layers and one or more core layers, wherein at least one core layer comprises the cellulose-containing material and the glue, and wherein the covering layers each comprise a cellulose-containing material and a glue based on carbohydrates and an amine containing hyperbranched polyamide, wherein the weight ratio of the hyperbranched polyamide to the cellulose-containing material in the covering layers is higher than the weight ratio of the hyperbranched polyamide to the cellulose-containing material in the last mentioned core layer. The weight ratio is preferably a weight ratio based on the weight of dry matter. Therefore, in the covering layers, the weight percentage of the hyperbranched polyamide relative to the cellulose-containing material can be, for example, 2 to 3, and in the core layer, the weight percentage of the hyperbranched polyamide relative to the cellulose-containing material can be 0.5 to 2. The glue used for the covering layers can be the same glue as the glue used for one or more of the core layers. However, other glues can also be used for various layers, but for example, always based on carbohydrates and amine glue. The board can be, for example, a 3-layer particle board, comprising two outer covering layers with less coarse wood chips and a core layer with coarser wood chips. The core layer can include recycled wood chips. Such particleboards can be produced, for example, using a press plate at a temperature of 170° C. to 245° C. at a pressure of 2 N / mm 2 Up to 5 N / mm 2 The cellulose-containing material of each layer may be made under a pressure of at least 3 seconds, preferably at least 5 seconds per millimeter of board thickness. The composition of the cellulose-containing material of each layer may be different. One or more core layers and / or cover layers may, for example, comprise recycled cellulose-containing material.
[0046] In a specific embodiment, the hyperbranched polyamide comprises a first group of hyperbranched polyamides and a second group of hyperbranched polyamides, wherein the average molecular weight of the first group of hyperbranched polyamides is at least 3 times higher than the average molecular weight of the second group of hyperbranched polyamides, preferably at least 5 times higher, and / or wherein the average molecular weight of the first group of hyperbranched polyamides is at most 15 times higher than the average molecular weight of the second group of hyperbranched polyamides, preferably at most 10 times higher. Here, the first group of hyperbranched polyamides forms a high molecular weight hyperbranched polyamide, and the second group of hyperbranched polyamides forms a low molecular weight hyperbranched polyamide. The combination of high molecular weight hyperbranched polyamides and low molecular weight hyperbranched polyamides improves the performance of the glue in terms of reactivity and technical characteristics. The high molecular weight hyperbranched polyamide has, for example, at least 5000, and preferably at least 10000 g / mol average molecular weight, for example 5000 g / mol to 50000 g / mol, preferably 10000 g / mol to 25000 g / mol average molecular weight. The low molecular weight polyamide has an average molecular weight of, for example, 500 g / mol to 5000 g / mol. By this combination, the further polymerization of the glue during the pressing of the board is accelerated. The pumpability of the glue is also better. The glue can also wet the cellulose-containing material better, so the distribution of the glue on the cellulose-containing material is better, and the gluing is also better. Here, we discuss a group of hyperbranched polyamides with an average molecular weight. Not all macromolecules from the same group have the same molecular weight. For example, this is the result of producing these hyperbranched polyamides. In the polycondensation of amino acids, not all amino acids will obtain the same reaction, i.e. the same branching, so the hyperbranched polyamides obtained have different molecular weights. The hyperbranched polyamides from the same group are obtained by, for example, the same production, wherein, for example, for the first group of hyperbranched polyamides, the polycondensation occurs for a longer time than the second group of hyperbranched polyamides, so the average molecular weight of the first group of hyperbranched polyamides is higher than the average molecular weight of the second group of hyperbranched polyamides. Preferably, the two groups of hyperbranched polyamides are obtained by two different productions. The average molecular weight of the hyperbranched polyamide can be determined, for example, by low angle laser light scattering (LALLS). Alternatively or in addition, the average molecular weight can be determined by gel permeation chromatography (GPC). Preferably, in this specification, the average molecular weight refers to the number average molecular weight.
[0047] More preferably, the second group of hyperbranched polyamides accounts for 5 wt % to 30 wt %, preferably 10 wt % to 20 wt %, of the total weight of the hyperbranched polyamides.
[0048] In a specific embodiment, the hyperbranched polyamide comprises almost exclusively high molecular weight hyperbranched polyamides, the average molecular weight of the hyperbranched polyamides being, for example, at least 5000 g / mol, and preferably at least 10000 g / mol, for example, the average molecular weight being 5000 g / mol to 50000 g / mol, preferably 10000 g / mol to 25000 g / mol. "Almost exclusively" means that if a second group of low molecular weight hyperbranched polyamides as indicated above is present and / or if low molecular weight hyperbranched polyamides (e.g. hyperbranched polyamides having a molecular weight of, for example, less than 5000 g / mol) are present, the weight percentage of the second group and / or low molecular weight hyperbranched polyamides relative to the total weight of the hyperbranched polyamides is preferably less than 0.1, preferably less than 0.05, even more preferably less than 0.005, and most preferably the second group is absent.
[0049] In a more preferred embodiment, the glue comprises an amine crosslinking agent, wherein preferably these amine crosslinking agents are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes. These amine crosslinking agents provide additional crosslinking between the hyperbranched polyamides during the board forming process, which ensures good performance of the formed board. These amine crosslinking agents, if for example they contain glyoxal and / or dialdehydes, also form part of the above-mentioned crosslinking agents. Therefore, the amine crosslinking agents can not only provide additional crosslinking between the hyperbranched polyamides, but also provide additional crosslinking in the Maillard reaction.
[0050] The amine crosslinking agent is or comprises, for example, a polyester, wherein these polyesters are preferably dispersed and / or unsaturated polyesters. These unsaturated polyesters are, for example, highly branched, so that they have good solubility and do not adversely affect the viscosity of the glue used to form the board. In processes where pressing is used to produce the board, the acidity of the polyester is preferably close to that of the polyamide or is stabilized so that there is no acid / base reaction before pressing, which would lead to undesirable prepolymerization.
[0051] The glue may comprise one or more types of amine crosslinkers. During the pressing of the board, these amine crosslinkers ensure better and faster gluing between the cellulose-containing materials, so that the obtained board has the necessary stiffness and strength, and the bond between the cellulose-containing materials does not break undesirably. In addition, by means of these amine crosslinkers, the pressing time can be further shortened and the technical properties of the finished product, such as particleboard, OSB or MDF, are improved. Technical characteristics are, for example, flexural strength, tensile strength, compressive strength and water resistance.
[0052] The amine crosslinking agent is or includes, for example, an epoxide. Excellent results can be obtained by epoxides, such as diepoxides or triepoxides or polyepoxides or combinations of various epoxides mentioned above. These epoxides, such as diepoxides or triepoxides, can, for example, contain one or more ethylene oxide end groups, and preferably contain two or more ethylene oxide end groups. These epoxides can, for example, be prepared by bio-based routes from lignin or aniline, such as glycerol diglycidyl ether and / or ethylene glycol diglycidyl ether. These epoxides can, for example, include diglycidyl ether of vanillyl alcohol and / or phloroglucinol triepoxide resins. Epoxides are known to react with amines. Therefore, tertiary amines are used as hardener components together with epoxy resins. However, after gluing of the cellulose-containing material and before pressing of the board, the hyperbranched polyamide can be contacted with the epoxide without undesirable prepolymerization, which is an exception. Preferably, the hyperbranched polyamide is contacted with the epoxide in an amount exceeding the stoichiometric amount. In the case of hyperbranched polyamides, the epoxide is mainly active only when the pressure and temperature are increased in the press. Adding epoxide to the hyperbranched polyamide hardly results in any increase in the viscosity of the glue. Therefore, the pressing of the board will not be hindered and very good bonding can be achieved between cellulose-containing materials. These amine crosslinking agents may have been mixed with the hyperbranched polyamide of the glue used in advance and can be stored like this. However, the amine crosslinking agent can also be combined shortly before gluing with the hyperbranched polyamide of the glue used. The glue used then is, for example, two-part, comprising a first part comprising the hyperbranched polyamide and a second part comprising the amine crosslinking agent, wherein the two parts are combined only before or during gluing of the cellulose-containing material. The amine crosslinking agent can also be considered as a separate component, separated from the glue used to produce the board, wherein the glue used then forms a cured glue based on the hyperbranched polyamide present in the board together with the amine crosslinking agent.
[0053] More preferably, the weight ratio of the amine crosslinker to the hyperbranched polyamide is 0.02 to 0.15, for example 0.02 to 0.08. Thus, for example 3 wt% to 7 wt% of epoxide or 3 wt% to 6 wt% of peroxide, for example 4 wt% or 5 wt% or 6 wt% of epoxide, may be present relative to the hyperbranched polyamide. A higher proportion of amine crosslinkers contributes to the water resistance of the glue and thus to the water resistance of the board containing such glue. The content of amine crosslinkers should also not be too high, as this may lead to prepolymerization of the glue before pressing the board. This weight ratio ensures optimal technical properties, more specifically better tensile strength, flexural strength and compressive strength and better water resistance. Therefore, this board is not only suitable for applications under dry indoor conditions (service class 1), but is also very suitable for wet spaces, such as wet indoor spaces (such as bathrooms) (service class 2). These boards can meet the current specifications of the relevant European standards EN 312, EN 300 or EN 622-5.
[0054] The amines for example account for 15 wt% to 50 wt%, preferably 30 wt% to 40 wt% of the total weight of the amines and carbohydrates. The carbohydrates then account for 50 wt% to 85 wt%, preferably 60 wt% to 70 wt% of the total weight of the amines and carbohydrates. The amines preferably comprise at least 80 wt%, preferably at least 90 wt%, and most preferably 95 wt% of hyperbranched polyamides, wherein these hyperbranched polyamides preferably have an average molecular weight higher than 500 g / mol, preferably higher than 5000 g / mol, and even more preferably higher than 10000 g / mol, and / or wherein these hyperbranched polyamides preferably have an average molecular weight lower than 100000 g / mol, even more preferably lower than 50000 g / mol, and most preferably lower than 25000 g / mol.
[0055] According to a third aspect, the present invention also relates to a glue for bonding cellulose-containing materials (such as plant fibers and / or wood chips and / or wooden parts) to form boards, wherein the glue is based on amines and carbohydrates, wherein the glue contains additives for controlling the Maillard reaction. This glue is a glue for making boards as described in the first aspect above. Therefore, the advantages and embodiments of the boards related to the glue shown above also apply to this glue. Surprisingly, it has been found that this glue is very suitable for gluing cellulose-containing materials such as wood fibers or other plant fibers, wood chips, wood layers and wood chips together to form boards by pressing. Here, the amines and carbohydrates form Maillard reactants, which react with each other during the Maillard reaction to form Maillard reaction products. This glue can also be used for impregnating paper to form impregnated paper. Such impregnated papers are very suitable for forming laminates comprising an MDF / HDF / chipboard substrate and one or more impregnated papers bonded to the substrate, or forming HPLs (High Pressure Laminates) consisting of two or more impregnated papers bonded together, or HPL boards (compact boards) comprising at least 5, preferably at least 10, even more preferably at least 15 impregnated papers bonded together. The present invention therefore relates to an impregnated paper impregnated with a glue as described above.
[0056] After curing, for example by pressing, the glue contains Maillard reaction products, which are derived from the Maillard reaction between the amines and the carbohydrates. The additive controls the Maillard reaction in the desired direction. The glue is based on the amines, carbohydrates and additives. This means that the amines, carbohydrates and additives will be provided during the glue formation process. The percentages, amounts and proportions of the amines, carbohydrates and additives are always expressed here based on the amount of dry matter provided for the formation of the glue. This is because during the glue formation process, before the glue is used to form a board, the amines and carbohydrates may have (partially) reacted with each other.
[0057] Additives may, for example, increase the reactivity of the glue and / or counteract undesired prepolymerization and / or increase the adhesion of the cured glue. Thus, additives provide a better glue.
[0058] The Maillard reaction is a general term for a series of complex chemical reactions that occur between reducing sugars and amines. Here, carbohydrates and amines form Maillard reactants. The additive may or may not be used for the Maillard reaction and may or may not form part of the Maillard reactants. One or more types of additives may be used.
[0059] Here, "amine" refers to a compound that contains at least one amine radical and is therefore a source of amine.
[0060] The amine, for example, accounts for 15 wt% to 50 wt% of the total weight of the amine and the carbohydrate, for example, 15 wt% to 40 wt%, preferably 20 wt% to 30 wt%. Then, the carbohydrate accounts for 50 wt% to 85 wt% of the total weight of the amine and the carbohydrate, preferably 70 wt% to 80 wt%. The amine may, for example, include a diamine such as hexamethylenediamine (HDMA) and / or a hyperbranched polyamide. The amine, for example, accounts for 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 35 wt%, 36 wt%, 37 wt% or 38 wt% of the total weight of the amine and the carbohydrate.
[0061] The carbohydrate is a reducing sugar and / or is converted into a reducing sugar. Reducing sugars are necessary for the Maillard reaction. Thus, sucrose can be used, which is converted into glucose and fructose. Sucrose is a widely available sugar and is a cheap bio-based carbohydrate source. The carbohydrate can also be invert sugar. The carbohydrate can also contain only glucose or only fructose. Thus, a 65 wt% to 75 wt% invert sugar aqueous solution, such as a 70 wt% invert sugar aqueous solution, can be used. The solution is then contacted with an amine.
[0062] Preferably, the additive comprises a base for adjusting the pH. By means of the base, the pH during the Maillard reaction is controlled, thereby achieving the formation of the desired Maillard reaction product. Surprisingly, it has been found that K2CO3 is a base that is very suitable for use as an additive. K2CO3 is a base that ensures a faster start of the Maillard reaction, but does not lead to an undesirable prepolymerization of the glue. Preferably, the base also comprises K2CO3, and even more preferably, the base comprises only K2CO3. Prepolymerization refers to the polymerization of the glue before, for example, the forming (e.g. pressing) of the board. Adding K2CO3 does not lead to an undesirable increase in the viscosity of the glue. Other bases may also be used, such as the strong bases NaOH and KOH. The base may also comprise Na2CO3 and / or Na2HPO4, for example comprising only one of these bases. NaOH and KOH may lead to undesirable prepolymerization, resulting in reduced technical properties of the board, so these are not very suitable. Two or more different bases may also be used.
[0063] More preferably, the alkali accounts for 0.05 wt% to 20 wt%, such as 1 wt% to 20 wt%, even more preferably 2 wt% to 10 wt%, and most preferably 3 wt% to 5 wt% of the glue dry matter content.
[0064] In a preferred embodiment, the additive comprises a salt of chloric acid, such as a salt of hypochlorous acid. Salts of hypochlorous acid promote the formation of Strecker degradation products during the Maillard reaction, so that a board with greater stiffness and / or less glue at the same stiffness can be obtained. Surprisingly, it was found that sodium hypochlorite (NaOCl) has a particularly positive effect. Therefore, the salt of hypochlorous acid preferably comprises NaOCl, and even more preferably NaOCl. Other possible salts of hypochlorous acid are potassium hypochlorite and calcium hypochlorite. In addition to or instead of the salt of chloric acid, chloric acid itself, such as, for example, HCl, can also be used.
[0065] More preferably, the salt of chloric acid, such as hypochlorous acid, comprises 0.12 to 20 wt%, such as 0.2 to 10 wt%, such as 1 to 20 wt% or 2 to 10 wt% or 3 to 4 wt% of the dry matter content of the gum.
[0066] Instead of (or in addition to) a salt of hypochlorous acid, HCl itself may also be added, wherein the additive then comprises HCl. When sucrose is used as carbohydrate and pre-reactant, HCl is a suitable additive, since the acid has a positive effect on the conversion of sucrose into glucose and fructose.
[0067] In a particularly preferred embodiment, the additive comprises a crosslinking agent, and these crosslinking agents are preferably intermediates formed in the Maillard reaction between an amine and a carbohydrate. In order to form the glue, the following substances will now be provided: the amine, the carbohydrate, and the additional crosslinking agent, which have not yet reacted with the reducing sugar. By means of these crosslinking agents, the reactivity of the glue and therefore the quality of the glue are improved. The crosslinking agent preferably comprises at least one aldehyde group and at least one carboxyl group. These crosslinking agents are both aldehydes and carboxylic acids. When the crosslinking agent is used for the Maillard reaction, these crosslinking agents are regarded as Maillard reactants. By actively adding the intermediates, i.e. the crosslinking agents, rather than waiting until these intermediates are formed during the Maillard reaction, it can be ensured that the various reaction pathways of the Maillard reaction are already directly present when the glue is first used.
[0068] More preferably, the crosslinking agent is selected from the group comprising α-hydroxyaldehydes, glyceraldehydes and α-dicarbonyl compounds. The best results are obtained with α-dicarbonyl compounds, since they have the most positive influence on the reactivity of the gum. These α-dicarbonyl compounds may be, for example, dialdehydes and / or glyoxal and / or methylglyoxal and / or deoxy-ketosugars. α-dicarbonyl compounds react with the amines present to form AGE products (advanced glycation end products), which may be classified as melanoidins if the molecular weight is above 10 kilodaltons. The crosslinking agent may be, for example, glyoxal.
[0069] When the cross-linking agent is an intermediate formed in the Maillard reaction between the amine and the carbohydrate, these intermediates may have an effect on the viscosity of the glue used to form the board. Therefore, during the formation of the glue, and therefore during the mixing of the various ingredients, this is preferably taken into account. Therefore, it can be chosen when to add these intermediates and / or how to mix. Therefore, these intermediates can be added during the formation of the above-mentioned pre-reactant.
[0070] More preferably, these crosslinking agents represent 0.3 wt % to 3 wt % of the gum, even more preferably 0.7 wt % to 1.6 wt % based on the dry matter content. Here, the weight percentage refers to the amount of dry matter of the crosslinking agent, such as the amount of α-dicarbonyl compound, such as the amount of dialdehyde and / or glyoxal and / or methylglyoxal and / or deoxy-ketoose added during the gum formation process.
[0071] Also more preferably, the ratio of α-dicarbonyl compounds, such as dialdehydes and / or glyoxal and / or methylglyoxal and / or deoxy-ketosugars to the total dry weight of amines and carbohydrates is 0.01 to 0.20, preferably 0.02 to 0.1. This ratio is related to the ingredients used in the glue formation process. In order to form the glue, glyoxal or another α-dicarbonyl compound is preferably prepared as an aqueous solution of, for example, at least 30 wt% of glyoxal (or another α-dicarbonyl compound) to facilitate addition and good mixing. Therefore, an aqueous solution containing 40 wt% of glyoxal or 50 wt% of glyoxal can be used to form the glue.
[0072] In a specific embodiment, the additive comprises a metal-containing component, such as a metal oxide and / or a metal hydroxide and / or a metal salt forming a chelate. The weight percentage of the metal-containing component relative to the cellulose-containing material is, for example, 0.01 to 0.2, preferably 0.025 to 0.1. In addition, the addition of Ca(OH)2, Mg(OH)2 or CaCl2 can solidify the polymer formed after the pressed board, which contributes to the stiffness and strength of the board.
[0073] In a specific embodiment, the additive comprises an amine crosslinker, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes.
[0074] The weight ratio of the amine crosslinking agent to the hyperbranched polyamide may be 0.02 to 0.15, for example, 0.02 to 0.08.
[0075] According to a fourth aspect, the present invention also relates to a glue, optionally as described in the third aspect above, for bonding cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, to form a board, wherein the glue is based on an amine and a carbohydrate, wherein at least a certain proportion of the amine is selected from the group comprising hyperbranched polyamides or chain amides; and wherein the amine preferably comprises a hyperbranched polyamide.
[0076] The glue is a glue for making a board, which includes a cured glue derived from a glue based on carbohydrates and amines, wherein the amines include hyperbranched polyamides and / or chain amides, as described in the second aspect above. Therefore, the advantages and embodiments of these boards are applicable to this glue. Surprisingly, it was found that this glue is very suitable for gluing cellulose-containing materials, such as wood fibers or other plant fibers, wood chips, wood layers and wood chips together to form boards by pressing. This glue can also be used for impregnating paper to form impregnated paper. This impregnated paper is very suitable for forming a laminate comprising an MDF / HDF / particleboard substrate and one or more impregnated papers bonded to the substrate, or forming an HPL (high pressure laminate) composed of two or more impregnated papers bonded together, or an HPL board (compact board) comprising at least 5, preferably at least 10, and even more preferably at least 15 impregnated papers bonded together. Therefore, the present invention relates to an impregnated paper impregnated with the above-mentioned glue.
[0077] Preferably, the amine comprises a hyperbranched polyamide, wherein the hyperbranched polyamide comprises at least 50 wt %, preferably at least 70 wt %, even more preferably 90 wt % of the amine. Thus, all amines may be hyperbranched polyamides.
[0078] These hyperbranched polyamides are preferably obtained by polycondensation of amino acids, wherein these amino acids are preferably selected from the group comprising arginine, glutamine, asparagine and lysine.
[0079] In a specific embodiment, the hyperbranched polyamide comprises a first group of hyperbranched polyamides having an average molecular weight of 500 g / mol to 100000 g / mol, preferably 5000 g / mol to 50000 g / mol, and even more preferably 10000 g / mol to 25000 g / mol, and the hyperbranched polyamide more preferably comprises a second group of hyperbranched polyamides, wherein the average molecular weight of the first group of hyperbranched polyamides is at least 3 times higher, preferably at least 5 times higher, than the average molecular weight of the second group of hyperbranched polyamides, and / or wherein the average molecular weight of the first group of hyperbranched polyamides is at most 15 times higher, preferably at most 10 times higher, than the average molecular weight of the second group of hyperbranched polyamides, and wherein, even more preferably, the second group of hyperbranched polyamides accounts for 5 wt% to 30 wt%, preferably 10 wt% to 20 wt%, of the total weight of the hyperbranched polyamides.
[0080] In a preferred embodiment, the glue comprises an amine crosslinker, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes, and wherein the weight ratio of the amine crosslinker to the hyperbranched polyamide is also preferably 0.02 to 0.15, for example 0.02 to 0.08. These amine crosslinkers provide additional crosslinking between the hyperbranched polyamides during the board forming process, which ensures the good performance of the formed board. These amine crosslinkers, if for example they contain glyoxal and / or dialdehydes, also form part of the above-mentioned crosslinker. Therefore, the amine crosslinker can not only provide additional crosslinking between the hyperbranched polyamides, but also provide additional crosslinking in the Maillard reaction. The amine crosslinker is or includes, for example, a polyester, wherein these polyesters are preferably dispersed polyesters and / or unsaturated polyesters. The amine crosslinker is or includes, for example, an epoxide. Excellent results are obtained by epoxides, such as diepoxides or triepoxides. These epoxides can be prepared, for example, by bio-based routes from lignin or aniline, such as glycerol diglycidyl ether and / or ethylene glycol diglycidyl ether.
[0081] For such glues, for embodiments not comprising any hyperbranched polyamide or comprising a hyperbranched polyamide, the weight ratio of the amine to the sum of the amine and the carbohydrate is preferably at most 0.4, and even more preferably at least 0.15. Thus, the weight ratio of the amine to the sum of the amine and the carbohydrate may be, for example: 0.22 or 0.23 or 0.24 or 0.25 or 0.26 or 0.27 or 0.28 or 0.35 or 0.36 or 0.37 or 0.38. When the amine is a hyperbranched polyamide, the weight ratio of the amine to the sum of the amine and the carbohydrate is, for example, 0.3 to 0.4.
[0082] The glue may comprise water as a solvent and / or may also be solvent-based. During the gluing of the cellulose-containing material, the water ensures that the cellulose-containing material is moistened and that the cell walls are even slightly penetrated. With the aid of such a glue, the cellulose-containing material can be well bonded together due to the good contact between the glue and the cellulose-containing material. By means of water as a solvent, the contact between the glue and the cellulose-containing material can be carried out at the level of almost the entire outer surface of the cellulose-containing material.
[0083] The viscosity of the glue used to form the board is preferably at most 20000 mPa.s, even more preferably at most 2000 mPa.s at 20°C and 1.013 bar.
[0084] The amines for example account for 15 wt% to 50 wt%, preferably 30 wt% to 40 wt%, of the total weight of the amines and carbohydrates. The carbohydrates then account for 50 wt% to 85 wt%, preferably 60 wt% to 70 wt%, of the total weight of the amines and carbohydrates. The amines preferably comprise at least 80 wt%, preferably at least 90 wt%, and most preferably 95 wt% of hyperbranched polyamides, wherein these hyperbranched polyamides preferably have an average molecular weight higher than 500 g / mol, preferably higher than 5000 g / mol, and even more preferably higher than 10000 g / mol, and / or wherein these hyperbranched polyamides preferably have an average molecular weight lower than 100000 g / mol, even more preferably lower than 50000 g / mol, and most preferably lower than 25000 g / mol.
[0085] The invention also relates to a method for forming a board comprising a cellulose-containing material such as plant fibers and / or wood chips and / or wooden parts, wherein a cellulose-containing material is provided and a glue is applied to the cellulose-containing material, after which the cellulose-containing material provided with the glue is pressed into a sheet material to form a board, wherein the glue is a glue as described above. By this method, a board is obtained as described in the first or second aspect. Therefore, all advantages and embodiments described above apply to this method. Surprisingly, pressing into a board can be carried out similarly to pressing a cellulose-containing material provided with a glue into a board, wherein the glue is a conventional UF glue.
[0086] Cellulose-containing materials, such as wood chips, wood fragments, wood layers, wood fibers or other plant fibers, are provided with glue and are glued, for example, by atomizing / spraying / pouring glue onto these cellulose-containing materials. Prior to this, the cellulose-containing materials can be placed in a gas stream or in a mixing container in order to glue the cellulose-containing materials as evenly as possible by atomization and / or mechanical friction. Then, for example, in a continuous press or a discontinuous press, the glue is pressed under a certain pressure, for example 2 N / mm 2 Up to 6 N / mm 2 , preferably 2 N / mm 2 Up to 4 N / mm 2The cellulose-containing material to be glued is compressed under a pressure of 100°C and at a temperature of, for example, 160°C to 245°C, preferably 200°C to 245°C, for a certain time, for example at least 4 seconds per millimeter of board thickness. The glue is then bonded to the cellulose-containing material and cured, thereby obtaining a strong board. This glue may be a single component, wherein the glue is stored as a whole and applied to the cellulose-containing material as a whole. The glue may also be a two-part or multi-part glue, wherein the glue comprises two or more different parts stored separately, wherein these parts are combined together before gluing, and thus applied to the cellulose-containing material as a whole, or wherein these parts are applied to the cellulose-containing material without prior combination, whether or not simultaneously.
[0087] In a specific embodiment, wherein the board comprises one or more layers, which are pressed together and at least one of said layers comprises said cellulose-containing material and said glue, wherein for this layer the weight ratio of glue to cellulose-containing material is from 0.03 to 0.15, preferably from 0.04 to 0.1. For example, the board may consist of three or more layers, namely outer cover layers and one or more core layers, wherein at least one core layer comprises said cellulose-containing material and said glue, and wherein the cover layers each comprise cellulose-containing material and the glue as indicated above, wherein the weight ratio of glue to cellulose-containing material in the cover layers is higher than the weight ratio of glue to cellulose-containing material in the last mentioned core layer.
[0088] In a specific embodiment, the glue comprises the crosslinking agent and / or the amine crosslinking agent, and / or the crosslinking agent and / or the amine crosslinking agent is applied to the cellulose-containing material. When the glue itself does not comprise the crosslinking agent and / or the amine crosslinking agent, the crosslinking agent and / or the amine crosslinking agent can be applied to the cellulose-containing material after gluing or during gluing. Preferably, the glue itself comprises the crosslinking agent and / or the amine crosslinking agent. By the crosslinking agent and / or the amine crosslinking agent, the polymerization during the pressing process is accelerated, so that the cellulose-containing material is bonded together faster. Therefore, the pressing time per millimeter of board thickness may be less than 10 seconds. These crosslinking agents and / or the amine crosslinking agents may or may not form part of the glue. Therefore, the glue may be a one-component glue, in which all components of the glue have been added to each other, and the glue is stored as such. The glue may also be a two-part or multi-part glue, in which the glue comprises two or more parts, which are combined before gluing, or applied to the cellulose-containing material together or continuously. In this way, undesirable prepolymerization can be avoided. The crosslinking agent and / or the amine crosslinking agent may also be considered as separate components which do not form any part of the glue.
[0089] In a preferred embodiment, the pressing is carried out at a temperature of 150°C to 250°C and 1.5 N / mm 2Up to 5 N / mm 2 The pressing is carried out under a pressure of at least 3 seconds per millimeter of board thickness. Depending on the pressing temperature and the type of press, the pressing time can be, for example, 3 to 7 seconds per millimeter of board thickness. Continuous or discontinuous presses can be used. Preferably, during the pressing process, water is sprayed onto the surface from below and above, for example 10 g / m 2 Up to 50 g / m 2 of water to facilitate heat transfer to the middle of the plate and reduce the total pressing time.
[0090] In a specific embodiment, the cellulose-containing material is coated with the glue by injection, spraying or by friction between the cellulose-containing materials or a combination of these techniques. Thus, a good gluing of the cellulose-containing material is obtained. This involves a similar or identical gluing as applied when using ordinary UF glues, so existing gluing steps of existing production processes do not need to be applied or only need to be applied to a limited extent to the glue according to the invention.
[0091] The invention also relates to a method for making a board glue, wherein an amine and a carbohydrate are provided, wherein the carbohydrate and a certain proportion of the amine are combined and heated to form a pre-reactant, after which the remaining amine is added to the pre-reactant, and wherein additives are provided, wherein these additives are added, for example, during the formation of the pre-reactant. The additive is an additive as described above, such as an alkali and / or an acid (such as HCl) and / or a salt of hypochlorous acid and / or a cross-linking agent and / or an amine cross-linking agent and / or a metal (hydr) oxide and / or a metal salt. The amine may include a hyperbranched polyamide as described above. This pre-reactant includes a carbohydrate and a certain proportion of the amine. The pre-reactant is preferably heated, for example, to a temperature of 50°C to 70°C, preferably 55°C to 65°C (and / or the carbohydrate and / or the proportion of the amine is heated before the combination to form the pre-reactant). In this way, the Maillard reaction occurs during the formation of the pre-reactant, and the pre-reactant already has a number of Maillard reaction products. The remaining amine is then added to form a glue, which is then used to glue cellulose-containing materials. The pre-reactant may also already contain a variety of additives or all additives. These additives can be added at the beginning of the pre-reactant formation, and can also be added during the pre-reactant formation process. In order to form the pre-reactant, for example, 5 wt% to 40 wt% of amine can be provided, for example, 15 wt% to 40 wt%, for example, 20 wt% to 30 wt%, for example, 10 wt% to 20 wt%, so that in the glue formed, there are still enough amines that have not yet reacted. Therefore, in the formation process of the pre-reactant, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt% or 18 wt% of amine can be added. Here, glue can be a two-component glue, wherein the pre-reactant constitutes a component of the glue, and the remaining amine (for example, hyperbranched amide) and the optional additive that is not added to the pre-reactant constitute the second component of the glue. The advantage here is that these two components can only be combined in a glue processing machine during the board forming process, so the undesirable prepolymerization risk is very small.
[0092] The present invention therefore relates to a two-component glue, wherein the glue is based on amines and carbohydrates, wherein at least a certain proportion of the amines is selected from the group comprising hyperbranched polyamides and chain amides; wherein the amines preferably comprise hyperbranched polyamides, and wherein the glue further comprises a first component and a second component, wherein the first component is a pre-reactant of at least substantially all of the carbohydrates and a certain proportion of the amines, and wherein the second component comprises the remaining amines. The first and / or second components may contain one or more or all of the above-mentioned additives, such as acids, bases, amine crosslinkers, crosslinking agents, salts, metal-containing components. For example, the first component may already contain epoxides and / or the second component may contain potassium carbonate. The amount of amine in the first component may be the amount of the above-mentioned pre-reactants. This glue can be used to bond cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, to form boards, but can also be used to impregnate paper.
[0093] An alternative embodiment of the invention relates to a glue for bonding insulating materials such as glass wool, rock wool, etc. to form, for example, a mat, wherein the glue is a glue as described above in the third or fourth aspect. The preferred embodiments of the glue as indicated above also apply to this alternative embodiment. With the aid of this glue, an insulating material such as glass wool, rock wool, etc. is then formed. Therefore, the present invention relates to an insulating material such as glass wool or rock wool, which comprises said glue based on an amine and a carbohydrate, and a method for producing an insulating material such as glass wool or rock wool, wherein said glue based on a carbohydrate and an amine is provided.
[0094] According to a variant embodiment, the present invention relates to a method for producing an alkaline raw material comprising amino acids, wherein the alkaline raw material can be used to produce hyperbranched polyamides, preferably by polycondensation of amino acids of the alkaline raw material. The alkaline raw material is preferably obtained by fermentation, wherein the fermentation is preferably carried out with bacteria. This alkaline raw material can be used to form a hyperbranched polyamide, for example by subjecting the amino acids present to polycondensation at a temperature (e.g., at 120°C to 180°C) for several hours, for example, in the presence of an optional catalyst and / or a strong base (e.g., KOH). Specific embodiments of the variant embodiments are presented in the following non-exhaustive list. Combinations of the features in this non-exhaustive list are possible, as long as they do not contradict each other:
[0095] Bacteria are provided which are capable of producing amino acids in a directed manner by fermentation. Thus, for example, bacteria can be provided which are capable of producing mainly lysine and, for example, in smaller amounts, one or more other amino acids, such as glutamine, wherein preferably the weight percentage of the other amino acids is at most 20%, preferably at most 10%, even more preferably at most 5% of the total amount of amino acids produced. Thus, these bacteria produce an alkaline raw material comprising amino acids, wherein this alkaline raw material can be described as a lysine source of industrial quality. The standards of lysine sources of industrial quality are lower than those of lysine sources for food or feed use;
[0096] The basic raw material comprises an amino acid selected from the group consisting of arginine, glutamine, asparagine and lysine. The basic raw material may comprise one, a combination of two, a combination of three or all amino acids from the above group;
[0097] The alkaline raw material comprising the amino acid is produced by bacterial fermentation, wherein for the fermentation one or more carbohydrate sources and one or more ammonium sources are provided. The one or more ammonium sources include, for example, one or more ammonium salts, such as ammonium sulfate or diammonium phosphate. The one or more carbohydrate sources include, for example, sucrose, glucose, cellulose, hemicellulose, starch or lignin. The carbohydrate source is, for example, molasses, starch hydrolysate, starch-containing wastewater, wood-containing sources, recycled sources such as recycled MDF or recycled particleboard. The result is, for example, an alkaline raw material in the form of a pulp, which pulp comprises the amino acids. A drying step of this pulp is not necessary. The production of hyperbranched polyamides can start without a prior drying step of the pulp or with a limited drying step;
[0098] The basic raw material containing amino acids is produced by bacterial fermentation. These bacteria can be, for example, Corynebacterium and / or E. coli bacteria;
[0099] The alkaline raw material is produced by bacterial strains that produce L-lysine. These bacterial strains may be, for example, Corynebacterium and / or E. coli bacteria;
[0100] The fermentation is carried out at a pH of 7 to 8, preferably 7.3 to 7.7 and / or a temperature of 28°C to 35°C, preferably 30°C to 33°C;
[0101] The fermentation is carried out in a reactor with an agitator: a "stirred tank reactor";
[0102] Fermentation is carried out in batch, fed-batch mode or continuous mode;
[0103] Additives are added to increase the yield of specific amino acids (such as L-lysine) during fermentation. DETAILED DESCRIPTION
[0104] In order to better illustrate the characteristics of the present invention, some preferred embodiments are described below as examples without any limiting characteristics.
[0105] A first example of a panel according to the invention is a 3-layer particleboard comprising two outer covering layers and a central layer. The central layer comprises coarse wood chips, which may or may not originate from wood waste and / or recycled particleboard, and the covering layers comprise finer wood chips. Here, the wood chips are bonded together by a glue based on carbohydrates, hyperbranched polyamides and additives. These additives include, among others, one or more of the following components: alkali, salts of hypochlorous acid and / or HCl, crosslinking agents as defined above, amine crosslinking agents as defined above. Additives include, for example, one or more of the following components: K2CO3, NaOCl and / or HCl, α-dicarbonyl compounds and epoxides. The gum may comprise, for example, the following weight percentages, based on dry matter content: 69% carbohydrates (e.g. sucrose), 23% hyperbranched polyamide, 4% K2CO3, 3% NaOCl and 1% glyoxal; or 59% carbohydrates (e.g. sucrose), 35% hyperbranched polyamide, 3.5% K2CO3, 0.5% HCl and 2% epoxide; or 69% carbohydrates (e.g. sucrose), 26.5% hyperbranched polyamide, 1% epoxide, 3% K2CO3 and 0.5% HCl; or 60.8% carbohydrates (e.g. sucrose), 36% hyperbranched polyamide, 2% epoxide, 1% K2CO3 and 0.2% HCl; or 59% carbohydrates (e.g. sucrose), 35% hyperbranched polyamide, 2% epoxide, 3.8% K2CO3 and 0.2% HCl. The composition of the glue of the center layer may or may not be the same as the composition of the glue of the cover layers.
[0106] A second example of a board according to the invention is a wood fiber board, such as an MDF or HDF board. Such a wood fiber board is single-layered and comprises wood fibers and a glue as defined in the above paragraph.
[0107] Hyperbranched polyamides are obtained by polycondensation of amino acids comprising mainly lysine. In addition to lysine, which is preferably L-lysine, there is, for example, a small amount of glutamine. Thus, glutamine, for example, accounts for up to 5 wt % of the amino acids present. The amino acids are derived from an alkaline raw material comprising amino acids. This alkaline raw material is obtained, for example, by bacterial fermentation, wherein these bacteria form lysine in a directed manner.
[0108] In a 3-layer particleboard, the glue of the different layers is, for example, the same glue. The cover layers use more glue than the central layer. This ensures that the cellulose-containing materials below the level of the cover layers do not undesirably loosen from each other. It is not superfluous to use more glue in the cover layers, since the cover layers consist of finer particles and therefore the total surface area to be glued is significantly increased.
[0109] Preferably, the operation is performed using the above-mentioned pre-reactants for forming the plate.
[0110] For illustrative purposes, some test results on particleboard are discussed below, demonstrating the advantages of various preferred embodiments of the present invention:
[0111] Two tests (tests 1 and 2) were carried out on a board containing a glue according to the prior art. This was to be able to compare a board according to the invention with a board according to the prior art. Then, 6 additional tests (tests 3 to 8) were carried out on a board according to the invention. For all the boards tested, the weight percentage of amine in the total weight of amine and carbohydrate was always 25%. For all these boards, the same type of chips and the same carbohydrate were used in order to obtain results that can be compared with each other. The same press and the same pressing temperature were generally used to form the boards. The boards had the same thickness. The amine in tests 1 to 6 was HDMA. The amine in tests 7 and 8 contained 24 wt% of HDMA and 76 wt% of hyperbranched polyamide. The density was measured according to EN 323, the thickness was measured according to EN 324-1 and the tensile strength was measured according to EN 319. The flexural strength and the modulus of elasticity were measured according to EN 310.
[0112]
[0113] With K2CO3, better tensile strength, flexural strength and elastic modulus were obtained. Among other things, better flexural strength and elastic modulus were obtained with glyoxal. With hyperbranched polyamides, high tensile strength and flexural strength were obtained.
Claims
1. A board comprising cellulose-containing materials such as plant fibers and / or wood chips and / or wooden parts, and a curing glue for bonding these cellulose-containing materials together, wherein the curing glue is derived from a glue based on amines and carbohydrates and the curing glue contains Maillard reaction products derived from a Maillard reaction between these amines and carbohydrates, characterized in that The gum contains additives for controlling the Maillard reaction.
2. The panel of claim 1, wherein the additive comprises a base.
3. The panel of claim 2, wherein the base comprises K2CO3.
4. A board according to claim 2 or 3, wherein the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the cured glue, wherein preferably, for this layer, the weight percentage of the alkali relative to the cellulose-containing material is 0.03 to 1, even more preferably 0.1 to 1, even more preferably 0.1 to 0.4, most preferably 0.15 to 0.
25.
5. A panel according to any one of the preceding claims, wherein the additive comprises a salt of chloric acid, such as a salt of hypochlorous acid.
6. The panel of claim 5, wherein the salt of chloric acid comprises sodium hypochlorite (NaOCl).
7. A board according to claim 5 or 6, wherein the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the cured glue, wherein preferably the weight percentage of the salt of hypochlorous acid in this layer relative to the cellulose-containing material is 0.01 to 1, such as 0.02 to 0.2 or 0.1 to 1 or 0.1 to 0.
2.
8. Panel according to any one of the preceding claims, wherein the additives comprise crosslinking agents, and these crosslinking agents are preferably intermediates formed in the Maillard reaction between amines and carbohydrates.
9. The panel according to claim 8, wherein the cross-linking agent is selected from the group consisting of alpha-hydroxyaldehydes, glyceraldehydes and alpha-dicarbonyl compounds.
10. A board according to claim 8 or 9, wherein the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the curing glue, wherein preferably, in this layer the weight percentage of the cross-linking agent relative to the cellulose-containing material is 0.02 to 0.16, preferably 0.04 to 0.
08.
11. A plate according to any one of the preceding claims, characterised in that The additive comprises a metal-containing component, such as a metal oxide and / or a metal hydroxide and / or a metal salt.
12. The panel according to any one of the preceding claims, wherein the additive comprises amine crosslinkers, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes.
13. A board according to claim 12, wherein the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the curing glue, wherein preferably for this layer the weight percentage of the amine cross-linking agent to the cellulose-containing material is 0.05 to 0.25, such as 0.07 to 0.
19.
14. A board, optionally according to any one or more of the preceding claims, comprising cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, and a curing glue for bonding these cellulose-containing materials together, wherein the curing glue is derived from a glue based on amines and carbohydrates, and the curing glue comprises Maillard reaction products derived from a Maillard reaction between these amines and carbohydrates, wherein at least a proportion of the amines is selected from the group comprising hyperbranched polyamides and chain amines; and wherein preferably at least a proportion of the amines is a hyperbranched polyamide.
15. The panel according to claim 14, wherein the amine comprises at least a hyperbranched polyamide, and preferably the hyperbranched polyamide comprises at least 50 wt%, preferably at least 70 wt% of the amine.
16. The panel according to claim 14 or 15, wherein the hyperbranched polyamide is obtained by polycondensation of amino acids, wherein these amino acids are preferably selected from the group comprising arginine, glutamine, asparagine and lysine.
17. The panel according to any one of claims 14 to 16, wherein the hyperbranched polyamide comprises a first group of hyperbranched polyamides having an average molecular weight of 500 to 100000 g / mol, preferably 5000 to 50000 g / mol and even more preferably 10000 to 25000 g / mol.
18. A board according to any one of claims 14 to 17, wherein the board comprises one or more layers, wherein at least one of the layers comprises the cellulose-containing material and the curing glue, wherein preferably in this layer the weight percentage of hyperbranched polyamide relative to the cellulose-containing material is 0.5 to 4, preferably 0.5 to 3, for example 1 to 2.
19. A sheet according to any one of claims 14 to 18, wherein the hyperbranched polyamide comprises a first group of hyperbranched polyamides and a second group of hyperbranched polyamides, wherein the average molecular weight of the first group of hyperbranched polyamides is at least 3 times higher, preferably at least 5 times higher, than the average molecular weight of the second group of hyperbranched polyamides, and / or wherein the average molecular weight of the first group of hyperbranched polyamides is at most 15 times higher, preferably at most 10 times higher, than the average molecular weight of the second group of hyperbranched polyamides.
20. The panel according to any one of claims 14 to 19, wherein the glue comprises amine crosslinkers, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes.
21. The panel of claim 20, wherein the weight ratio of amine crosslinker to hyperbranched polyamide is from 0.02 to 0.
15.
22. A glue for bonding cellulose-containing materials such as plant fibers and / or wood chips and / or wooden parts to form boards, wherein the glue is based on amines and carbohydrates, characterized in that The gum contains additives for controlling the Maillard reaction.
23. The gum according to claim 22, wherein the additive comprises a base for adjusting the pH.
24. A glue according to claim 23, wherein the base comprises K2CO3.
25. Gum according to claim 23 or 24, wherein the base comprises 0.5 wt% to 20 wt%, such as 1 wt% to 20 wt%, such as 3 wt% to 5 wt%, based on the dry matter content of the gum.
26. Glue according to any one of claims 22 to 25, wherein the additive comprises a salt of chloric acid, such as a salt of hypochlorous acid.
27. The glue of claim 26, wherein the salt of chloric acid comprises sodium hypochlorite (NaOCl).
28. Glue according to claim 26 or 27, wherein the salt of hypochlorous acid comprises 0.1 wt% to 20 wt%, such as 0.2 wt% to 10 wt%, such as 1 wt% to 20 wt%, based on the dry matter content of the glue.
29. A gum according to any one of claims 22 to 28, wherein the additive comprises crosslinking agents, and these crosslinking agents are preferably intermediates formed during the Maillard reaction between amines and carbohydrates.
30. The gum according to claim 29, wherein the cross-linking agent is selected from the group comprising alpha-hydroxyaldehydes, glyceraldehydes and alpha-dicarbonyl compounds.
31. A gum according to claim 29 or 30, wherein the cross-linking agent comprises 0.3 wt% to 3 wt% based on the dry matter content of the gum.
32. Glue according to any one of claims 22 to 31, wherein the additive comprises a metal-containing component, such as a metal oxide and / or a metal hydroxide and / or a metal salt.
33. Glue according to claims 22 to 32, wherein the additive comprises amine crosslinkers, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes, and wherein also preferably the weight ratio of amine crosslinker to hyperbranched polyamide is from 0.02 to 0.
15.
34. A gum according to claims 22 to 33 wherein the weight ratio of amine to the total weight of amine and carbohydrate is at most 0.4, and preferably at least 0.
15.
35. A glue for bonding cellulose-containing materials such as plant fibers and / or wood chips and / or wooden parts to form boards, optionally according to any one or more of claims 22 to 34, wherein the glue is based on an amine and a carbohydrate, wherein at least a proportion of the amine is selected from the group comprising hyperbranched polyamides and chain amides; wherein the amine preferably comprises a hyperbranched polyamide.
36. The gum according to claim 35, wherein the amine comprises a hyperbranched polyamide, and wherein the hyperbranched polyamide comprises at least 50 wt%, preferably at least 70 wt%, even more preferably at least 90 wt% of the amine.
37. Gum according to claim 35 or 36, wherein the hyperbranched polyamide is obtained by polycondensation of amino acids, wherein these amino acids are preferably selected from the group comprising arginine, glutamine, asparagine and lysine.
38. Glue according to any one of claims 35 to 37, wherein the hyperbranched polyamide comprises a first group of hyperbranched polyamides having an average molecular weight of 500 g / mol to 100000 g / mol, preferably 5000 g / mol to 50000 g / mol and even more preferably 10000 g / mol to 25000 g / mol, and wherein preferably the hyperbranched polyamide comprises a second group of hyperbranched polyamides, wherein the average molecular weight of the first group of hyperbranched polyamides is at least 3 times higher, preferably at least 5 times higher, than the average molecular weight of the second group of hyperbranched polyamides, and / or wherein the average molecular weight of the first group of hyperbranched polyamides is at most 15 times higher, preferably at most 10 times higher, than the average molecular weight of the second group of hyperbranched polyamides, and wherein more preferably the second group of hyperbranched polyamides represents 5 to 30 wt%, preferably 10 to 20 wt%, of the total weight of the hyperbranched polyamides.
39. Glue according to any one of claims 35 to 38, wherein the glue comprises amine crosslinkers, wherein preferably these amine crosslinkers are selected from the group comprising polyketones, polyesters, isocyanate dispersions, epoxides, glyoxal and other dialdehydes, and wherein also preferably the weight ratio of amine crosslinker to the hyperbranched polyamide is from 0.02 to 0.
15.
40. A gum according to any one of claims 22 to 39 wherein the weight ratio of amine to the total weight of amine and carbohydrate is at most 0.4, and preferably at least 0.
15.
41. A method for forming a board comprising cellulose-containing materials, such as plant fibers and / or wood chips and / or wooden parts, wherein cellulose-containing materials are provided and glue is applied to these cellulose-containing materials, after which these cellulose-containing materials provided with glue are pressed into sheet-like materials to form the board, characterized in that The glue is a glue according to any one or more of claims 22 to 40.
42. A method according to claim 41, wherein the board comprises one or more layers, wherein the layers are pressed together, and wherein at least one of the layers comprises the cellulose-containing material and the glue, wherein for this layer the weight ratio of glue to cellulose-containing material is from 0.03 to 0.
10.
43. The method according to claim 41 or 42, wherein the pressing is performed at a temperature of 150°C to 250°C and 1.5 N / mm 2 Up to 5 N / mm 2 The pressure is applied for at least 3 seconds per millimeter of plate thickness.
44. A method for making board glue, wherein an amine and a carbohydrate are provided, wherein the carbohydrate and a proportion of the amine are combined and heated to form a pre-reactant, after which the remainder of the amine is added to the pre-reactant, characterized in that Additives are provided, wherein these additives are added, for example, before the pre-reactant is formed, during the pre-reactant is formed, or after the pre-reactant is formed.
Citation Information
Patent Citations
Adhesive
CN106103630A
Binders
CN106661418A
Wood particle boards
CN108349106A
Preparation method of semi-solid bamboo liquid-protein hot pressboard glue
CN108795377A
Tough soybean meal protein adhesive and preparation method thereof
CN109679578A