Ossein scaffold material loaded with multiple growth factors and preparation method of ossein scaffold material

Through collagen stent materials loaded with multiple growth factors, the problems of poor mechanical properties and fast degradation speed of bone replacement materials in periodontitis treatment are solved, and the bone regeneration effect is improved and the appropriate treatment cycle is achieved, and the biosafety is good and degradation effects.

CN119034011APending Publication Date: 2024-11-29BEIJING YILING BIOTECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192704.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The bone replacement materials in the treatment of existing periodontitis have poor mechanical properties and fast degradation speed, making it difficult to effectively promote the growth of oral osteoblasts, resulting in poor bone regeneration effect.

Method used

Develop a collagen scaffold material loading multiple growth factors. By treating naturally-derived animal bones, it can improve mechanical properties and osteoinduction capabilities by loading growth factors such as FGF, VEGF, TGF-β, and BMP. , prolongs the degradation time, suitable for the treatment of periodontitis.

Benefits of technology

It improves the mechanical properties and osteoinduction ability of the collagen stent, extends the degradation time, promotes the growth of oral osteoblasts and bone regeneration, is suitable for the treatment cycle of periodontitis, and has good biosafety and degradation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034011A_ABST
    Figure CN119034011A_ABST
Patent Text Reader

Abstract

The invention discloses an ossein scaffold material loaded with multiple growth factors and a preparation method of the ossein scaffold material. The ossein scaffold material comprises an acellular matrix for promoting growth of oral osteoblasts and the multiple growth factors loaded on the acellular matrix. The acellular matrix is a bone collagen scaffold obtained from animal bones which contain collagen and are naturally sourced; the multiple growth factors are FGF, VEGF, TGF-beta and BMP. The collagen scaffold material disclosed by the invention is subjected to secondary freeze-drying, so that the collagen content is higher, the collagen scaffold material has a good surface void aperture, the mechanical property is ensured, the bone induction capability is improved, the collagen scaffold material is suitable for loading various growth factors, and the degradation time is prolonged so as to adapt to the treatment effect of periodontitis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomedicine, and in particular relates to a collagen scaffold material loaded with multiple growth factors and a preparation method thereof. Background Art

[0002] Periodontitis, also known as destructive periodontal disease, is a chronic inflammatory disease that is mainly caused by the destruction of periodontal tissues by bacteria in dental plaque. Periodontitis can lead to the destruction of periodontal supporting tissues (gingiva, periodontal ligament, alveolar bone and cementum), the formation of periodontal pockets (small pockets formed by the widening of the gap between teeth and gums), loss of attachment and absorption of alveolar bone. As the disease progresses, the teeth will gradually loosen, and gum recession can eventually lead to tooth loss. Oral implant restoration is currently the preferred method of restoration for patients with edentulous / missing teeth, but the alveolar bone in the implant area often atrophies, which can lead to insufficient bone mass in the alveolar bone and can easily have a significant impact on the restoration effect.

[0003] According to incomplete statistics, the proportion of adults in my country suffering from periodontitis is as high as over 60%. At present, guided bone tissue regeneration technology is the mainstream procedure for auxiliary treatment, which mainly promotes new bone formation by implanting bone substitutes or other biological materials at the site of periodontal bone loss. The bone substitute materials currently used in clinical practice are roughly divided into artificial synthetic materials and biological bone materials. Among them, artificial synthetic materials have the problem of difficult to control degradation rate, which leads to poor bone regeneration effect. Most of the biological bone materials currently used in clinical practice are pure inorganic substances extracted from three-dimensional heterogeneous carbonate apatite crystals after removing the organic components from bovine bones, such as the finished product Bio-oss artificial bone powder provided by Geistlich of Switzerland and OSHAIS of the United States; the bone powder has a relatively simple composition and does not contain any organic components. It has the problems of poor mechanical properties and fast degradation rate.

[0004] Therefore, seeking biomass materials with good mechanical properties and degradation speed that can be suitable for bone defect filling and promote the growth of oral osteoblasts remains a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above problems and purposes, the present invention proposes a collagen scaffold material loaded with multiple growth factors and a preparation method thereof, wherein the collagen scaffold obtained by processing animal bones from natural sources is loaded with multiple growth factors to improve mechanical properties and bone induction ability, prolong degradation time, and is suitable for the treatment cycle of periodontitis. The specific technical scheme is as follows:

[0006] First, the present invention provides a collagen scaffold material loaded with multiple growth factors, the collagen scaffold material includes a decellularized matrix for promoting the growth of oral osteoblasts and multiple growth factors loaded on the decellularized matrix; the decellularized matrix is ​​a collagen scaffold obtained from animal bones of natural origin containing collagen; the multiple growth factors are selected from two or more of FGF, VEGF, TGF-β, and BMP.

[0007] The aforementioned collagen scaffold material loaded with multiple growth factors comprises 80wt% to 98wt% collagen and 2wt% to 10wt% miscellaneous proteins, and the rest is hydroxyapatite.

[0008] Preferably, in the aforementioned collagen scaffold material loaded with multiple growth factors, the total protein content of the collagen scaffold is 84.22wt% to 98.53wt%.

[0009] Further preferably, the aforementioned collagen scaffold material loaded with multiple growth factors comprises 96.74wt% collagen and 1.79wt% miscellaneous proteins, and the pore size of the surface pores is 60-70 μm.

[0010] The aforementioned collagen scaffold material loaded with multiple growth factors contains four growth factors: FGF, VEGF, TGF-β, and BMP, and the loading amounts thereof are respectively:

[0011] FGF 20~27ng / g,

[0012] VEGF 18~25ng / g,

[0013] TGF-β26~32ng / g,

[0014] BMP 24~30ng / g.

[0015] The aforementioned collagen scaffold material loaded with multiple growth factors has a wet compressive strength of 0.0120 to 0.0221 MPa and a dry compressive strength of 1.25 to 2.90 MPa.

[0016] Secondly, the present invention provides a method for preparing the aforementioned collagen scaffold material loaded with multiple growth factors, comprising the following steps:

[0017] 1) Preparing a collagen scaffold: removing fat from the surface of the animal bone, pouring it into a cleaning box and placing it in a constant temperature oscillator for defatting, then drying and crushing it and soaking it in a protease solution for 30 to 60 minutes, then washing it in an acidic solution for 8 to 10 times and filtering it out, and finally soaking it in purified water for 24 to 48 hours, draining it, and freeze-drying it to obtain a collagen scaffold;

[0018] 2) Growth factor loading: The collagen scaffold prepared in step 1) is crushed again to a particle size of 1 to 10 μm, then immersed in a growth factor solution for 12 to 24 hours, centrifuged, the supernatant is discarded, poured into a mold for freeze drying, packaged and irradiated for sterilization to obtain a collagen scaffold material.

[0019] As a preferred technical solution, the aforementioned method for preparing a collagen scaffold material loaded with multiple growth factors, in step 1), prepare a collagen scaffold, the degreasing solution is a mixture of dichloromethane or chloroform and methanol, and the degreasing parameters are: temperature: 5-45°C; rotation speed: 300-600rpm; the degreasing solution is a mixture of dichloromethane or chloroform and methanol, and the solid-liquid ratio is 1:3-5.

[0020] As a preferred technical solution, the aforementioned method for preparing a collagen scaffold material loaded with multiple growth factors, in step 1), prepare a collagen scaffold, the acidic solution is hydrochloric acid and / or phosphoric acid, and its concentration is 0.5-1 mol / L; the purified water immersion temperature is 0°C, and the purified water is changed every 12 hours during the immersion process. When changing the water, its pH is detected, and a pH value of 6-7.5 is qualified.

[0021] As a preferred technical solution, in the aforementioned method for preparing a collagen scaffold material loaded with multiple growth factors, in step 2), the concentration of the growth factor loading growth factor solution is:

[0022] FGF: 30~50ng / ml,

[0023] VEGF: 25-40 ng / ml,

[0024] TGF-β: 40~65ng / ml,

[0025] BMP: 40-65 ng / ml;

[0026] The collagen scaffold is added with a growth factor solution, with a solid-liquid ratio of 1:5-10;

[0027] The soaking temperature is 0°C;

[0028] The radiation sterilization dosage is 10 to 30 kGy.

[0029] The beneficial effects of the present invention are:

[0030] 1) The collagen scaffold material of the present invention uses a collagen scaffold that is washed and defatted by a constant temperature oscillator, which reduces the use of chemical reagents and has better biosafety after multiple cleanings with no residual reagents;

[0031] 2) The collagen scaffold material of the present invention improves the bone induction ability and prolongs the degradation time by loading growth factors; among them: FGF promotes the synthesis of collagen and non-collagen by bone cells, VEGF effectively promotes the differentiation of osteoblasts and thus directly promotes osteogenesis, TGF-β changes the phenotype of normal fibroblasts, and BMP is effective for vertical bone defects and has the strongest bone induction ability; the four are used in combination, VEGF and FGF promote angiogenesis; BMP-2 and TGF-β jointly participate in bone regeneration and repair by regulating the proliferation and differentiation of osteoblasts; VEGF improves blood supply by promoting angiogenesis and enhances the bone induction effect of BMP-2; TGF-β can upregulate the expression of VEGF and enhance its activity, and can jointly regulate the process of bone repair and regeneration with VEGF, FGF, and BMP-2 to achieve the purpose of promoting bone regeneration, and with the participation of new blood vessels, a better regional osteogenesis effect can be achieved.

[0032] 3) The collagen scaffold material of the present invention has a higher collagen content through secondary freeze-drying, which can better promote bone regeneration. The surface of the collagen scaffold material has a suitable pore size, making it more suitable for cell climbing, achieving good mechanical properties and degradation rate while being suitable for bone defect filling and promoting the growth of oral osteoblasts.

[0033] 4) The collagen scaffold material of the present invention is sterilized by low-dose irradiation during packaging, which achieves the sterilization effect without destroying the growth factor structure, thereby ensuring that the mechanical properties, bone induction ability and degradation time of the product are not affected. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The SEM analysis results (500 μm) of the collagen scaffold material loaded with multiple growth factors of the present invention. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments and drawings.

[0036] Example 1

[0037] This embodiment is to prepare a collagen scaffold material loaded with multiple growth factors. The details are as follows:

[0038] Preliminarily remove the fat on the surface of the animal bones, and use purified water to wash the raw materials after fat removal until no grease overflows. Pour the washed raw materials into a cleaning box and put them into a constant temperature oscillator for degreasing, temperature: 30°C; rotation speed: 500rpm; the solution must completely cover the raw materials, (the solution is a chloroform-methanol solution, the volume ratio of chloroform to methanol is, chloroform: methanol = 1:5) the material-liquid ratio is 1:3, soak for 22.5 hours, take out after soaking and wash with running purified water 5 times, then put it into a vacuum drying oven for 6 hours, put the defatted raw materials into a grinder, use a filter to preliminarily sieve, and then immerse in the protease solution for 60 minutes, put it into the acidic solution to wash 10 times and filter it out, the acidic solution is hydrochloric acid, the concentration is 0.9mol / L. Then,

[0039] Use purified water to soak the raw materials at 0℃ for 42 hours, change the purified water every 12 hours, check the pH value when changing the water for the last time, the pH value is 7, drain the raw materials and put them into a freeze dryer.

[0040] The raw material is freeze-dried and then crushed twice to a particle size of 5 μm. The crushed raw material is immersed in a growth factor solution with the concentrations of FGF: 32 ng / ml, VEGF: 230 ng / ml, TGF-β: 49 ng / ml, and BMP: 44 ng / ml. The solution is mixed evenly with a material-liquid ratio of 1:6. After soaking at 0°C for 20 hours, the solution is centrifuged, the supernatant is discarded, the solution is poured into a mold for freeze-drying, and the solution is irradiated and sterilized (15 kGy) after packaging to obtain a collagen scaffold material loaded with multiple growth factors.

[0041] The growth factor loading of the collagen scaffold material is: FGF 25ng / g, VEGF 20ng / g, TGF-β30ng / g, BMP 28ng / g. SEM analysis shows that the pore size of the surface of the collagen scaffold material is 68μm. Figure 1 shown.

[0042] Example 2

[0043] This example is to investigate the effect of secondary freeze-drying on the pore size formation on the surface of the collagen scaffold material and its effect on the mechanical properties.

[0044] At the same time, the comparative sample 1 was prepared without secondary freeze-drying, and the existing bone powder (Geistlich, specification model: 50 mg) was used as the comparative sample 2. The specific preparation method is as follows:

[0045] The other steps are the same as those in Example 1, except that the material is not subjected to secondary pulverization after freeze-drying. After the last water change, the pH is detected. When the pH is 7, the material is drained and directly immersed in a growth factor solution. After immersion, the material is directly freeze-dried and sterilized by irradiation after packaging.

[0046] In this embodiment, the wet and dry compressive strength of the prepared collagen scaffold material is used as the inspection index. The specific detection method is: pour the comparative sample 1 prepared in Example 1 and this embodiment and the existing bone powder into the same mold (or cut) into samples of the same size 8*8*8 (unit: mm), and use a vernier caliper to measure the length, width and thickness of the sample with an accuracy of 0.01mm. Use a single-column desktop testing machine to cut the upper and lower bottom surfaces of the sample in contact with the equipment flat. The area of ​​the lower bottom surface in contact with the equipment is S (S=LW). Set the sample deformation to 5mm on the testing machine software, and conduct the test at a speed of 10mm / min. When the testing machine stops, record the sample force value F and calculate the compressive strength P=F / S. The results are shown in Table 1:

[0047] Table 1. Effects of different surface pore sizes on the mechanical properties of collagen scaffold materials

[0048] sample Drying method Pore ​​size (μm) Wet compressive strength (MPa) Dry compressive strength (MPa) Example 1 Secondary freeze drying 68μm 0.0221MPa 2.905MPa Comparative sample 1 One freeze-drying 79μm 0.0181MPa 1.905MPa Existing bone meal Other ways 43μm 0.00314MPa 3.180MPa

[0049] From the results in Table 1, it can be seen that the scaffold after crushing and secondary freeze-drying has a pore size of 68μm, its wet compressive strength is 0.0221Mpa, and its dry compressive strength is 2.90Mpa. It has good porosity and appropriate density, and can load growth factors well while providing appropriate support; the surface pore size of the comparative sample 1 prepared by secondary crushing without freeze-drying is 79μm, which is too loose, with a wet compressive strength of 0.0181MPa and a dry compressive strength of 1.905Mpa. The support is insufficient and the degradation time requirement is not met; and the surface pore size of the comparative sample 2 prepared by the existing bone powder is 79μm, which is too dense, with a wet compressive strength of 0.00314MPa and a dry compressive strength of 3.180MPa. The support is high enough, but the degradation time will be longer, which is not conducive to new bone growth and cannot match the periodontitis treatment cycle well.

[0050] Example 3

[0051] This example investigates the effect of growth factor content on the degradation time of collagen scaffold materials.

[0052] The collagen scaffold materials investigated in this example are consistent with those in Example 1 except for the different growth factor contents. The growth factor contents of various collagen scaffold materials are shown in Table 2.

[0053] The degradation time of collagen scaffold materials can be investigated by referring to:

[0054] YY / T0474-2004 In vitro degradation test of poly (L-lactide) resin and its products for surgical implants.

[0055] GB / T16886.9-2001 Biological evaluation of medical devices Part 9 Qualitative and quantitative framework for potential degradation products,

[0056] GB / T16886.13-2001 Biological evaluation of medical devices Part 13: Qualitative and quantitative determination of degradation products of polymer medical devices.

[0057] The specific degradation body experimental process is as follows:

[0058] The immersion solution (phosphate buffer: Sorensen buffer) contains potassium dihydrogen phosphate and disodium hydrogen phosphate prepared with sterile double distilled water. The salts used to prepare the above buffer are analytically pure and dried to a constant weight.

[0059] a) 1 / 15 mol / L potassium dihydrogen phosphate: dissolve 9.078 g potassium dihydrogen phosphate per liter of water;

[0060] b) 1 / 15mol / L disodium hydrogen phosphate: dissolve 11.876g disodium hydrogen phosphate dihydrate in each liter of water;

[0061] The soaking solution is a mixture of 18.2% solution a) and 81.8% solution b) (volume fraction).

[0062] The concentration of type I collagenase added to the soaking solution is 1.25 U / ml, and the pH value of the buffer solution is 7.4±0.2.

[0063] Place the test sample in a container, cover the sample with the prepared soaking solution and seal the container. The test sample is completely immersed in the soaking solution, and each sample uses about 20 ml of soaking solution. A constant temperature water bath or oven is used to maintain the test sample at a physiological temperature of (37±1)°C to simulate in vivo degradation. The complete degradation time of the sample is recorded. The results are shown in Table 2.

[0064] The growth factor content of each collagen scaffold material and its in vivo degradation time are shown in Table 2.

[0065] Table 2. Effects of different growth factor contents on the degradation time of collagen scaffold materials

[0066]

[0067] From the results in Table 2, it can be seen that the stents with growth factor content within the range value have a good degradation effect; when the content is lower than the range value, the stent degradation time becomes shorter, which is difficult to meet clinical needs; when the content is higher than the range value, the stent degradation time is too long, and there is a chance of cell proliferation, which is not conducive to the subsequent treatment of patients.

[0068] Example 4

[0069] This example is to test the biosafety of the collagen scaffold material prepared in Example 1.

[0070] In this example, the prepared collagen scaffold material is used as an experiment and extracted with polar extract and non-polar extract, and the presence of toxic substances in the solution at different extraction times is checked as an indicator. The detection method is carried out according to GB / T16886.11-2021 "Biological Evaluation of Medical Devices Part 11: Systemic Toxicity Test", and the results are shown in Table 3.

[0071] Table 3. Effect of the biosafety of the collagen scaffold material prepared by the preparation method of the present invention

[0072] Observation time sample Polar extract Non-polar extract immediately Example 1 AN AN 4h Example 1 AN AN 24h Example 1 AN AN 48h Example 1 AN AN 72h Example 1 AN AN

[0073] Note: AN = normal performance

[0074] It can be seen from the results in Table 3 that the collagen scaffold material prepared by the preparation method of the present invention has good biosafety and can be used for the treatment of periodontitis to guide bone tissue regeneration.

[0075] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view. In addition, it should be understood that although this specification is described in accordance with the implementation mode, it does not include only one technical solution. This narrative mode of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole, and the technical solutions in the embodiments can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A collagen scaffold material loaded with multiple growth factors, characterized in that: The collagen scaffold material includes a decellularized matrix for promoting the growth of oral osteoblasts and a plurality of growth factors loaded on the decellularized matrix; The decellularized matrix is ​​a collagen scaffold obtained from natural animal bones containing collagen; The multiple growth factors are selected from two or more of FGF, VEGF, TGF-β, and BMP.

2. The collagen scaffold material loaded with multiple growth factors according to claim 1, characterized in that: The collagen scaffold contains 80wt% to 98wt% collagen and 2wt% to 10wt% miscellaneous protein, and the rest is hydroxyapatite.

3. The collagen scaffold material loaded with multiple growth factors according to claim 2, characterized in that: The total protein content of the collagen scaffold is 84.22 wt% to 98.53 wt%.

4. The collagen scaffold material loaded with multiple growth factors according to claim 3, characterized in that: The collagen scaffold contains 96.74 wt % of collagen and 1.79 wt % of miscellaneous proteins, and the pore diameter of the surface pores is 60-70 μm.

5. The collagen scaffold material loaded with multiple growth factors according to claim 1, characterized in that: The collagen scaffold material contains four growth factors: FGF, VEGF, TGF-β, and BMP, and their loading amounts are: FGF 20~27ng / g, VEGF 18~25ng / g, TGF-β 26~32ng / g, BMP 24~30ng / g.

6. The collagen scaffold material loaded with multiple growth factors according to claim 1, characterized in that: The collagen scaffold material has a wet compressive strength of 0.0120-0.0221 MPa and a dry compressive strength of 1.25-2.90 MPa.

7. A method for preparing a collagen scaffold material loaded with multiple growth factors according to any one of claims 1 to 6, characterized in that: The steps include: 1) Preparation of collagen scaffold: remove fat from the surface of animal bones, pour them into a cleaning box and place them in a constant temperature oscillator for defatting, then dry and crush them and soak them in a protease solution for 30 to 60 minutes, then wash them in an acid solution for 8 to 10 times and filter them out, finally soak them in purified water for 24 to 48 hours, drain them, and freeze-dry them to obtain the collagen scaffold; 2) Growth factor loading: The collagen scaffold prepared in step 1) is crushed again to a particle size of 1 to 10 μm, and then immersed in a growth factor solution for 12 to 24 hours, centrifuged, the supernatant is discarded, poured into a mold for freeze-drying, packaged, and irradiated for sterilization to obtain a collagen scaffold material.

8. The method for preparing a collagen scaffold material loaded with multiple growth factors according to claim 7, characterized in that: In step 1), a collagen scaffold is prepared, the degreasing solution is a mixture of dichloromethane or chloroform and methanol, and the degreasing parameters are: temperature: 5-45°C; Rotation speed: 300-600rpm; the degreasing solution is a mixture of dichloromethane or chloroform and methanol, and the material-liquid ratio is 1:3-5.

9. The method for preparing a collagen scaffold material loaded with multiple growth factors according to claim 7, characterized in that: In step 1), a collagen scaffold is prepared, the acidic solution is hydrochloric acid and / or phosphoric acid, and the concentration thereof is 0.5-1 mol / L; the purified water immersion temperature is 0°C, and the purified water is changed every 12 hours during the immersion process. When the water is changed, its pH is detected, and a pH value of 6-7.5 is qualified.

10. The method for preparing a collagen scaffold material loaded with multiple growth factors according to claim 7, characterized in that: In step 2), the growth factor loading, the concentration of the growth factor solution is: FGF: 30~50ng / ml, VEGF: 25-40 ng / ml, TGF-β: 40~65ng / ml, BMP: 40-65 ng / ml; The collagen scaffold is added with a growth factor solution, with a solid-liquid ratio of 1:5-10; The soaking temperature is 0°C; The radiation sterilization dosage is 10 to 30 kGy.