Preparation method of absorbable internal fixation bone lamella

Through the composite material of polylactic acid and zinc-based alloy, high-tough bone plates are prepared by using hot pressing and molding technology, which solves the problems of large rigidity and poor bending resistance of fracture internal fixation materials, and realizes the high toughness and osteogenic characteristics of the bone plates , reducing the pain and financial burden of patients.

CN119034022AInactive Publication Date: 2024-11-29SHANDONG BRANDEN MEDICAL DEVICE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411545484.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing fracture internal fixation materials have high rigidity and poor bending resistance, which may lead to osteoporosis and secondary fractures, and are non-degradable, increasing the pain and financial burden of patients.

Method used

Polylactic acid is used as the matrix and zinc-based alloy is the reinforcement. High-toughness absorbable internal fixed bone plates are prepared through hot pressing, microarc oxidation and molding technology, and combined with milling and processing to improve the mechanical properties and osteogenic characteristics of the bone plates.

Benefits of technology

It improves the bending performance and toughness of the bone plate, promotes the proliferation of osteoblasts, reduces the risk of local inflammation, and degrades in the body, reducing the need for secondary surgery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034022A_ABST
    Figure CN119034022A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an absorbable internal fixation bone lamella, and belongs to the technical field of medical instruments. The absorbable internal fixation bone plate is prepared from a composite material, and takes polylactic acid as a matrix and a zinc-based alloy as a reinforcement. The preparation method comprises the following steps: (1) drying polylactic acid granules, and carrying out hot pressing to prepare polylactic acid slices; (2) stretching the zinc-based alloy wire, performing micro-arc oxidation treatment on the zinc-based alloy wire, and directionally arranging the zinc-based alloy wire; (3) dissolving polylactic acid, adding the dissolved polylactic acid to the zinc-based alloy wire, and evaporating a solvent to form a polylactic acid / zinc-based alloy composite sheet; (4) alternately stacking the polylactic acid sheets and the polylactic acid / zinc-based alloy composite sheets formed in the previous two steps, and carrying out compression molding to prepare a void-free plate; and (5) milling to obtain the absorbable internal fixation bone plate. The absorbable internal fixation bone plate prepared by the method has high toughness and osteogenesis characteristics, and is expected to solve the problems of poor mechanical property and cell affinity of the absorbable internal fixation bone plate clinically.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an absorbable internal fixation bone plate, and belongs to the technical field of medical devices. Background Art

[0002] With the increasing number of cars and industrial development in the world, there are a large number of traumatic fractures caused by traffic accidents and production safety accidents every year. Clinically, the incidence of fractures caused by aging, disease and severe trauma is high, and the selection of bone plates for repairing bone tissue damage has always been a medical problem. Traditional fracture internal fixation materials are generally made of stainless steel, titanium and their alloys, but these metal internal fixators have obvious defects. Since the rigidity of the implant material is much greater than that of cortical bone, it is affected by the "stress shielding" effect, and long-term implantation often leads to osteoporosis and induces secondary fractures; it may release toxic metal ions and microparticles under the action of physiological corrosion and wear, which can easily lead to adverse reactions such as tissue inflammation; in addition, this non-degradable material requires a second surgery to remove after bone healing, which increases the patient's pain and economic burden.

[0003] In recent years, biodegradable materials have attracted extensive attention from researchers due to their good biological properties. Compared with metal implants, the most clinically attractive advantage of this type of material is that it can be degraded in vivo during the bone repair process. After bone healing, there is no need for secondary removal surgery, which can reduce the risk of local inflammation that may occur due to long-term implantation. The current bone repair materials have entered the degradable era. Polylactic acid (PLA) has good biocompatibility and biodegradability. Its degradation products are glycolic acid and lactic acid, which can participate in the metabolic cycle of carbohydrates in the body. After a series of biochemical reactions, it is finally degraded into carbon dioxide and water and excreted from the body. It is one of the biodegradable polymers certified by the US Food and Drug Administration and has been widely used in drug controlled release systems, orthopedic fixation, tissue engineering scaffold materials, surgical sutures and other fields. The single PLA material has high rigidity and poor bending resistance, which leads to high brittleness and easy breakage in application scenarios requiring toughness. In addition, PLA also has the disadvantage of poor cell adhesion.

[0004] Patent application number CN200310110496.X discloses a composite material for bioabsorbable internal fixation devices and a preparation method thereof, wherein polylactic acid, polyglycolic acid, tricalcium phosphate, apatite, and carbon fiber are molded or extruded into rods and plates in a powder state or in the presence of an organic solvent or in a molten state, and then machined to obtain an orthopedic internal fixation device, with a bending strength of 175-355MPa and a shear strength of 80-186MPa. The carbon fiber is non-degradable and has a risk of infection if it exists in the body for a long time. Patent application number CN201210402262.1 discloses a PLA absorbable bone nail with PBC as a toughening agent and a preparation method thereof, wherein PLA, PBC, and HAP materials are melt-blended and then injection molded, and the toughening effect thereof is unknown. Patent application number CN201010557114.8 discloses a controllable degradation internal bone fixation composite material and its preparation method, which is composed of polylactic acid, nanorod-shaped hydroxyapatite particles and magnesium particles, and is formed into an absorbable bone nail by injection molding. Its preparation method is complicated and the toughening effect is unknown. Therefore, the present invention uses polylactic acid as a matrix and zinc-based alloy as a reinforcement to prepare an absorbable internal fixation bone plate with high toughness and osteogenic properties. Summary of the invention

[0005] The invention provides a preparation method of an absorbable internal fixation bone plate, so as to solve the problems of large rigidity and poor bending resistance of the current internal fixation bone plate, and develop an absorbable internal fixation bone plate with high toughness and osteogenic properties.

[0006] In order to achieve the above technical objectives, the present invention provides a method for preparing an absorbable internal fixation bone plate, comprising the following steps: (1) drying the polylactic acid pellets and hot pressing them to form polylactic acid sheets; (2) Directionally stretching the zinc-based alloy wire, performing micro-arc oxidation treatment, and then aligning it; (3) dissolving polylactic acid in a solvent, and then adding the polylactic acid to the zinc-based alloy wire treated in step (2), and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet; (4) alternately stacking the polylactic acid sheets prepared in step (1) and the polylactic acid / zinc-based alloy composite sheets prepared in step (3) to form a void-free plate by compression molding; (5) Obtain absorbable internal fixation bone plate through milling.

[0007] Furthermore, the polylactic acid pellets in step (1) are poly-L-lactic acid, and the molecular weight distribution range is 50,000-250,000.

[0008] Furthermore, in step (1), the hot pressing temperature range is 180-200° C., the pressure range is 0.3-0.5 MPa, and the time is 1-2 min.

[0009] Furthermore, in step (2), the zinc-based alloy wire comprises zinc and magnesium, wherein the mass fraction of magnesium is 0.5%-3%.

[0010] Furthermore, in step (2), the diameter of the zinc-based alloy wire is 0.2-0.4 mm, and the diameter of the zinc-based alloy wire after stretching is 0.1-0.3 mm.

[0011] Furthermore, the spacing between the directionally arranged zinc-based alloy wires in step (2) should be no greater than 0.05 mm.

[0012] Furthermore, the solvent in step (3) is dichloromethane, and the ratio of polylactic acid to the solvent is 1:40 (w / v).

[0013] Furthermore, the alternating stacking structure in step (4) is a structure of polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet.

[0014] Furthermore, the temperature in the compression molding in step (4) is 180-210° C., the pressure is 0.6-0.8 MPa, and the time is 1-2 min.

[0015] Through the above technical solution, a high-toughness absorbable internal fixation bone plate is prepared.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The absorbable internal fixation bone plate provided by the present invention is made of composite material, with polylactic acid as the matrix and zinc-based alloy wire as the reinforcement. The directional zinc-based alloy wire is combined with the polylactic acid matrix through compression molding technology. The introduction of zinc-based alloy improves the bending performance of the absorbable internal fixation bone plate and improves the toughness of the bone plate. This structural design is conducive to enhancing the mechanical properties of the absorbable internal fixation bone plate.

[0018] 2. The presence of zinc in zinc-based alloys can promote osteoblast proliferation, and the addition of copper can improve the mechanical properties of zinc-based alloys.

[0019] 3. Micro-arc oxidation treatment of the surface of zinc-based alloy wire is beneficial to improving the surface roughness and enhancing the interfacial bonding strength between the zinc-based alloy wire and the polylactic acid substrate.

[0020] In conclusion, the absorbable internal fixation bone plate prepared by this preparation method not only has high toughness, but also can promote the proliferation of osteoblasts and has potential osteogenic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of a method for preparing an absorbable internal fixation bone plate.

[0022] Figure 2 It is a schematic diagram of the structure of polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet.

[0023] Figure 3 Schematic diagram of a plate without voids.

[0024] In the figure, 1-polylactic acid sheet, 2-polylactic acid / zinc-based alloy composite sheet, 3-zinc-based alloy wire, 4-void-free plate. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] like Figure 1 The preparation flow chart of absorbable internal fixation bone plate. First, the polylactic acid pellets are dried, and then hot-pressed under high temperature and high pressure to form a polylactic acid sheet 1, and the hot-pressing parameters are as follows: the temperature range is 180-200°C, the pressure range is 0.3-0.5MPa, and the hot-pressing time is 1-2min; the zinc-based alloy wire 3 is directional stretched to a diameter of 0.1-0.3mm, and then subjected to micro-arc oxidation treatment; the zinc-based alloy wire 3 after directional arrangement treatment is arranged so that the interval between adjacent zinc-based alloy wires 3 is not greater than 0.05mm; the polylactic acid is dissolved in a solvent, and after dissolution, the solution is poured on the zinc-based alloy wire 3, and the solvent is evaporated to form a polylactic acid / zinc-based alloy composite sheet 2; the polylactic acid sheet 1 and the polylactic acid / zinc-based alloy composite sheet 2 formed in the first two steps are alternately stacked to form a polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet ( Figure 2 ); a void-free plate 4 is formed by compression molding ( Figure 3 ), the temperature is 180-210℃, the pressure is 0.6-0.8 MPa, and the hot pressing time is 1-2min; finally, the absorbable internal fixation bone plate is obtained by milling.

[0027] Example 1

[0028] The absorbable internal fixation bone plate is prepared according to the following steps:

[0029] (1) First, polylactic acid pellets with a molecular weight of 50,000 to 150,000 are dried, and then hot-pressed at 180° C. and 0.3 MPa for 1 min to form a polylactic acid sheet 1.

[0030] (2) The zinc-based alloy wire 3 (Cu content of 0.5%) was oriented and stretched to a diameter of 0.1 mm, and then subjected to micro-arc oxidation treatment: the electrolyte was a mixed solution of 10 g / L sodium silicate and 2 g / L sodium hydroxide, the voltage was 380 V, the frequency was 2000 Hz, and the time was 20 min; the treated zinc alloy wires 3 were oriented so that the interval between adjacent zinc-based alloy wires 3 was no more than 0.05 mm.

[0031] (3) dissolving polylactic acid in dichloromethane, wherein the ratio of polylactic acid to dichloromethane is 1:40 (w / v); after dissolution, pouring the solution onto the zinc-based alloy wire 3, and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet 2.

[0032] (4) The prepared polylactic acid sheet 1 and the polylactic acid / zinc-based alloy composite sheet 2 are alternately stacked to form a polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet structure; and a void-free plate is formed by compression molding at a temperature of 180°C, a pressure of 0.6 MPa, and a hot pressing time of 1 min.

[0033] (5) Finally, a customized tool is used to mill the gap-free plate to obtain a basically formed bone plate, and then the surface is finely processed to obtain an absorbable internal fixation bone plate.

[0034] Example 2

[0035] The absorbable internal fixation bone plate is prepared according to the following steps:

[0036] (1) First, polylactic acid pellets with a molecular weight of 150,000 to 250,000 are dried, and then hot-pressed at 190° C. and 0.4 MPa for 1.5 min to form a polylactic acid sheet 1.

[0037] (2) The zinc-based alloy wire 3 (Cu content of 1.75%) was oriented and stretched to a diameter of 0.2 mm, and then subjected to micro-arc oxidation treatment: the electrolyte was a mixed solution of 15 g / L sodium silicate and 3 g / L sodium hydroxide, the voltage was 420 V, the frequency was 2000 Hz, and the time was 20 min; the zinc-based alloy wires 3 after the oriented arrangement treatment were arranged so that the interval between adjacent zinc-based alloy wires 3 was no more than 0.05 mm.

[0038] (3) dissolving polylactic acid in dichloromethane, wherein the ratio of polylactic acid to dichloromethane is 1:40 (w / v); after dissolution, pouring the solution onto the zinc-based alloy wire 3, and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet 2.

[0039] (4) The prepared polylactic acid sheet 1 and the polylactic acid / zinc-based alloy composite sheet 2 are alternately stacked to form a polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet structure; and a void-free plate is formed by compression molding at a temperature of 195°C, a pressure of 0.7 MPa, and a hot pressing time of 1.5 min.

[0040] (5) Finally, a customized tool is used to mill the gap-free plate to obtain a basically formed bone plate, and then the surface is finely processed to obtain an absorbable internal fixation bone plate.

[0041] Example 3

[0042] The absorbable internal fixation bone plate is prepared according to the following steps:

[0043] (1) First, polylactic acid pellets with a molecular weight of 150,000 to 250,000 are dried, and then hot-pressed at 200° C. and 0.5 MPa for 2 minutes to form a polylactic acid sheet 1.

[0044] (2) The zinc-based alloy wire 3 (Cu content is 3%) is oriented and stretched to a diameter of 0.3 mm, and then subjected to micro-arc oxidation treatment: the electrolyte is a mixed solution of 18 g / L sodium silicate and 4 g / L sodium hydroxide, the voltage is 450 V, the frequency is 2000 Hz, and the time is 20 min; the treated zinc alloy wires 3 are oriented so that the interval between adjacent zinc-based alloy wires 3 is no more than 0.05 mm.

[0045] (3) dissolving polylactic acid in dichloromethane, wherein the ratio of polylactic acid to dichloromethane is 1:40 (w / v); after dissolution, pouring the solution onto the zinc-based alloy wire 3, and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet 2.

[0046] (4) The prepared polylactic acid sheet 1 and the polylactic acid / zinc-based alloy composite sheet 2 are alternately stacked to form a polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet structure; and a void-free plate is formed by compression molding at a temperature of 210°C, a pressure of 0.8 MPa, and a hot pressing time of 2 min.

[0047] (5) Finally, a customized tool is used to mill the gap-free plate to obtain a basically formed bone plate, and then the surface is finely processed to obtain an absorbable internal fixation bone plate.

[0048] Comparative Example 1

[0049] The absorbable internal fixation bone plate is prepared according to the following steps:

[0050] First, polylactic acid pellets with a molecular weight of 50,000 to 150,000 are dried, and then hot-pressed at 180° C. and 0.3 MPa for 1 minute to form a polylactic acid sheet 1. Then, an absorbable internal fixation bone plate is obtained by milling.

[0051] Comparative Example 2

[0052] The absorbable internal fixation bone plate is prepared according to the following steps:

[0053] (1) First, polylactic acid pellets with a molecular weight of 150,000 to 250,000 are dried, and then hot-pressed at 190° C. and 0.4 MPa for 1.5 min to form a polylactic acid sheet 1.

[0054] (2) The pure zinc wire is oriented and stretched to a diameter of 0.2 mm, and then subjected to micro-arc oxidation treatment: the electrolyte is a mixed solution of 15 g / L sodium silicate and 3 g / L sodium hydroxide, the voltage is 420 V, the frequency is 2000 Hz, and the time is 20 min; the treated zinc alloy wires 3 are oriented and arranged so that the interval between adjacent zinc-based alloy wires 3 is no more than 0.05 mm.

[0055] (3) dissolving polylactic acid in dichloromethane, wherein the ratio of polylactic acid to dichloromethane is 1:40 (w / v); after dissolution, pouring the solution onto the zinc-based alloy wire 3, and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet 2.

[0056] (4) The prepared polylactic acid sheet 1 and the polylactic acid / zinc-based alloy composite sheet 2 are alternately stacked to form a polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet structure; and a void-free plate is formed by compression molding at a temperature of 195°C, a pressure of 0.7 MPa, and a hot pressing time of 1.5 min.

[0057] (5) Finally, a customized tool is used to mill the gap-free plate to obtain a basically formed bone plate, and then the surface is finely processed to obtain an absorbable internal fixation bone plate.

[0058] 1. Mechanical properties test

[0059] The same specification and model of bone plates (straight bone plates, length 18mm, width 5mm, thickness 2mm, number of holes 4) produced in the embodiment and the comparative example were tested for mechanical properties, and the bending strength of the product was tested with reference to the test method provided in the national standard YY / T0509-2009, and the bending moment when the bone plate was bent to 0.2% offset displacement was tested (if the bone plate has broken before reaching the specified displacement, the bending moment at the time of the break is defined as the bending strength). The test results are shown in Table 1.

[0060] Table 1 Bending strength (N)

[0061] Bending strength (N) Example 1 169 Example 2 178 Example 3 166 Comparative Example 1 82 Comparative Example 2 135

[0062] According to the data in Table 1, it can be seen that the bending strength of the embodiment is between 166-178N, while the bone plate of the comparative example 1 product has broken before reaching the specified displacement. In comparative example 2, pure zinc alloy wire is used as a reinforcement, and its bending strength is not as good as that of the embodiment. This shows that the absorbable internal fixation bone plate of the embodiment has good toughness.

[0063] 2. In vitro degradation experiment

[0064] The test was carried out according to the method provided in standard YY / T 0474-2004, and the mass retention rates of the embodiments and comparative examples after 3 months of biodegradation were calculated, as shown in Table 2.

[0065] Table 2 Quality retention rate (%)

[0066] Quality retention rate (%) Example 1 98.22 Example 2 98.54 Example 3 98.15 Comparative Example 1 95.23 Comparative Example 2 97.76

[0067] From the data in Table 2, it can be seen that the mass retention rate of the embodiment after 3 months of degradation is 98.15-98.54%, which is higher than that of the comparative example, and the degradation rate in the initial stage of the action is lower than that of the comparative example.

[0068] 3. Effect of absorbable internal fixation bone plate extract on osteoblast proliferation

[0069] Preparation of extract: The absorbable internal fixation bone plates in the examples and comparative examples were disinfected and sterilized, phosphate buffer solution (PBS) was added at a ratio of 0.2 g / mL, the pH of the solution was adjusted to 7.2, and after 72 h at 37°C, the PBS after soaking the three groups of materials was collected under sterile conditions, and the extracts of each group of materials were aseptically retained.

[0070] Take MC3T3-E1 cells with good growth status and prepare a cell suspension. Add 200 μL of 1×10 5 / L cell suspension was inoculated into a 96-well plate. After culturing for 24 h, osteoblasts were treated with the extract and the medium was changed every 2 days. 2 The cells were cultured in the incubator for 1 d, 3 d, and 7 d. The extract was discarded, the cells were washed with PBS, 20 μL of CCK-8 solution was added, and the cells were cultured for another 4 h. The optical density (OD) at 450 nm was measured with an enzyme-linked immunosorbent assay, and the relative growth rate was calculated. The relative growth rate (%) = OD of the experimental group / OD of the blank control group × 100%.

[0071] Table 3 Relative value-added rate (%)

[0072] project Day 1 Day 3 Day 7 Example 1 92.56±1.53 93.24±2.35 99.52±2.92 Example 2 96.23±0.67 98.11±1.86 105.42±2.41 Example 3 94.62±0.85 94.63±2.52 101.67±2.77 Comparative Example 1 97.23±0.39 96.55±1.63 94.12±2.25 Comparative Example 2 95.45±0.51 97.59±1.86 102.58±2.93

[0073] Table 3 is the CCK-8 test results, which show that the relative proliferation rate of osteoblasts in Example 2 and Comparative Example 2 increases with time, and the difference is statistically significant (P<0.05); while the relative proliferation rate of osteoblasts in Comparative Example 1 decreases with time, and the absorbable internal fixation bone plate of the present application has the effect of promoting the proliferation of osteoblasts.

Claims

1. A method for preparing an absorbable internal fixation bone plate, It is characterized in that The following steps are involved: (1) drying the polylactic acid pellets and then hot pressing them to make polylactic acid sheets; (2) The zinc-based alloy wire is stretched and then subjected to micro-arc oxidation treatment, and then oriented; (3) dissolving polylactic acid in a solvent, and then adding the polylactic acid to the zinc-based alloy wire treated in step (2), and evaporating the solvent to form a polylactic acid / zinc-based alloy composite sheet; (4) alternately stacking the polylactic acid sheets prepared in step (1) and the polylactic acid / zinc-based alloy composite sheets prepared in step (3) to form a void-free plate by compression molding; (5) Obtain absorbable internal fixation bone plate through milling.

2. A method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The polylactic acid pellets in step (1) are poly-L-lactic acid, and the molecular weight distribution range is 50,000-250,000.

3. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The hot pressing temperature in step (1) is 180-200° C., the pressure is 0.3-0.5 MPa, and the time is 1-2 min.

4. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The zinc-based alloy wire in step (2) comprises zinc and copper, wherein the mass fraction of copper is 0.5%-3%.

5. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The diameter of the zinc-based alloy wire in step (2) is 0.2-0.4 mm, and the diameter of the zinc-based alloy wire after the stretching treatment is 0.1-0.3 mm.

6. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The spacing between the zinc-based alloy wires arranged in a direction in the step (2) should be no greater than 0.05 mm.

7. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The solvent in step (3) is dichloromethane, and the ratio of polylactic acid to the solvent is 1:40 (w / v).

8. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The alternately stacked structure in step (4) is a structure of polylactic acid sheet-polylactic acid / zinc-based alloy composite sheet-polylactic acid sheet.

9. The method for preparing an absorbable internal fixation bone plate according to claim 1, It is characterized in that The compression molding in step (4) is performed at a temperature of 180-210° C., a pressure of 0.6-0.8 MPa, and a time of 1-2 min.

Citation Information

Patent Citations

  • Mg-containing high-strength deforming zinc-copper alloy and preparation method thereof

    CN101906554A

  • Bio-absorbable medical compound material and preparation method thereof

    CN102397589A

  • Magnesium alloy sheet-reinforced absorbable intrabony fixing composite material and preparation method thereof

    CN102552993A

  • Solution-treated absorbable zinc-copper-alloy ligating clip and preparation method thereof

    CN110916747A

  • Long-time efficient antibacterial full-degradable medical zinc alloy / polylactic acid composite material and preparation method thereof

    CN116531575A