Desulfurizing agent and preparation method thereof

By preparing active iron oxide and hydroxy iron oxide seed crystals, combined with structural additives and metal additives, the problems of high cost of desulfurizer and insufficient sulfur capacity in the steel industry are solved, and high sulfur capacity, easy to form and multiple times can be prepared. Recycled desulfurizer meets the strict gas purification requirements of the steel industry.

CN119034465APending Publication Date: 2024-11-29JIZHI WISDOM (SHANGHAI) NEW TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411402302.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing desulfurizers in the steel industry are costly and have insufficient sulfur capacity, making them difficult to meet the increasingly stringent gas purification requirements, and there are shortcomings in molding and regeneration of iron-based desulfurizers in room temperature.

Method used

By preparing active iron oxide and iron hydroxyoxide seed crystals, combined with specific structural additives and metal additives, desulfurization agents are prepared by drying and calcining steps to reduce production costs and at the same time improve the sulfur capacity and porosity of the desulfurization agent.

Benefits of technology

It realizes high sulfur capacity, easy molding and multiple regeneration desulfurizer, reduces production costs and improves desulfurization capacity, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005075617230000101
    Figure BDA0005075617230000101
  • Figure BDA0005075617230000111
    Figure BDA0005075617230000111
Patent Text Reader

Abstract

The invention discloses a desulfurizing agent and a preparation method thereof. The preparation method comprises the following steps: 1) preparing active iron oxide: adding alkali into an iron-based raw material, carrying out neutralization reaction at 100-150 DEG C to form ferric hydroxide, and drying ferric hydroxide precipitate to obtain the active iron oxide; (2) preparing a ferric oxyhydroxide seed crystal: stirring a mixed solution of soluble ferrite and a precipitant, curing to obtain a reaction product, and carrying out solid-liquid separation on the reaction product to obtain the ferric oxyhydroxide seed crystal; wherein the molar ratio of ferrous ions to hydroxyl ions in the mixed solution is (1: 0.7)-(1: 1.5); and 3) mixing the active iron oxide, the iron oxyhydroxide seed crystal, a binder, a structural auxiliary agent and a metal auxiliary agent, molding, drying, and roasting at 300-550 DEG C for 1-8 hours to obtain the desulfurizer. The desulfurizer prepared by the invention has relatively large porosity and pore volume, and high sulfur capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a desulfurizing agent and a preparation method thereof. Background Art

[0002] It is estimated that the annual sulfur dioxide emissions in the steel industry can reach 1.06 million tons, accounting for 7% of the total emissions of key industrial enterprises. High emissions from the steel industry are the main cause of air pollution, so all production links in the steel industry urgently need to carry out ultra-low emission transformation to promote the improvement of environmental air quality.

[0003] In order to meet the increasingly stringent requirements for gas purification, technicians in this field have conducted various studies on dry fine desulfurizers in recent years. Room-temperature iron-based desulfurizers have the advantages of wide sources, large sulfur capacity, and easy regeneration. They are widely used and effective dry room-temperature desulfurizers. Common desulfurizers include iron oxide desulfurizers and hydroxy iron desulfurizers.

[0004] CN107684819A discloses a composite iron-based desulfurizer. The raw material composition of the desulfurizer is: 60-80 parts of iron oxyhydroxide, 20-40 parts of basic zinc carbonate, and 0.5-1.2 parts of a binder. The desulfurizer can be used for gas desulfurization under high space velocity conditions, and has high desulfurization accuracy and high desulfurization efficiency, but the cost of basic zinc carbonate is relatively high, which increases the desulfurization cost.

[0005] CN114643056A discloses a high sulfur capacity iron oxyhydroxide desulfurization catalyst, which is composed of the following components in percentage by mass: 50% to 90% iron oxyhydroxide and 10% to 50% auxiliary agent. The auxiliary agent is at least one of white clay, carboxymethyl cellulose, calcium-based bentonite, high-alumina cement, attapulgite, sesbania powder, calcium sulfate dihydrate and pseudo-boehmite. The iron oxyhydroxide desulfurization catalyst has the advantages of high sulfur capacity, high desulfurization accuracy and high desulfurization performance. However, the desulfurization catalyst is fine particles, which are difficult to shape and expensive. Summary of the invention

[0006] In view of this, one object of the present invention is to provide a method for preparing a desulfurizer, which not only saves the production cost of the desulfurizer, but also maintains a high sulfur capacity of the desulfurizer. Another object of the present invention is to provide a desulfurizer prepared by the above method.

[0007] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.

[0008] In one aspect, the present invention provides a method for preparing a desulfurizing agent, comprising the following steps:

[0009] 1) Preparation of activated iron oxide: adding alkali to an iron-based raw material, performing a neutralization reaction at 100-150° C. to form iron hydroxide, and drying the iron hydroxide precipitate to obtain activated iron oxide;

[0010] 2) preparing ferric oxyhydroxide seed crystals: stirring a mixed solution of a soluble ferrous salt and a precipitant, aging the solution to obtain a reaction product, and separating the reaction product into a solid and liquid to obtain ferric oxyhydroxide seed crystals; wherein the molar ratio of ferrous ions to hydroxide ions in the mixed solution is 1:0.7 to 1:1.5;

[0011] 3) Mixing active iron oxide, iron oxyhydroxide seed crystals, a binder, a structural additive and a metal additive, drying, and calcining at 300-550° C. for 1-8 hours to obtain a desulfurizer; wherein the structural additive comprises, by weight, 4-8 parts by weight of diatomaceous earth, 2.5-5 parts by weight of ammonium bicarbonate, and 2-6 parts by weight of polystyrene microspheres.

[0012] According to the preparation method of the present invention, preferably, an oxidizing atmosphere is blown into the neutralization reaction.

[0013] According to the preparation method of the present invention, preferably, the base in step 1) is selected from at least one of ammonia water, sodium hydroxide, sodium carbonate and sodium bicarbonate.

[0014] According to the preparation method of the present invention, preferably, the pH value of the mixed solution in step 2) is 7-9, the aging temperature is 20-40° C., and the aging time is 2-10 h.

[0015] According to the preparation method of the present invention, preferably, in step 2), the soluble ferrous salt is selected from at least one of ferrous sulfate, ferrous chloride, ferrous nitrate and ferrous acetate;

[0016] The precipitant is selected from at least one of ammonia water, sodium hydroxide, calcium hydroxide and sodium carbonate.

[0017] According to the preparation method of the present invention, preferably, the drying in step 3) is carried out in an oxidizing atmosphere, the drying temperature is 80-120° C., and the drying time is 1-10 h.

[0018] According to the preparation method of the present invention, preferably, in step 3), the sum of the activated iron oxide and the hydroxy iron oxyde crystal seeds is 42 to 86.5 parts by weight, the binder is 3 to 26 parts by weight, the structural additive is 8.5 to 24 parts by weight and the metal additive is 2 to 8 parts by weight, wherein the weight ratio of the activated iron oxide to the hydroxy iron oxyde crystal seeds is 1:1 to 1:5.

[0019] According to the preparation method of the present invention, preferably, the binder is selected from at least one of gypsum, lime, calcium silicate, cement and polyvinyl alcohol;

[0020] The metal additive is selected from at least one of an alkali metal salt, an alkaline earth metal salt and a transition metal salt;

[0021] The structural auxiliary agent also includes at least one of bentonite and urea.

[0022] According to the preparation method of the present invention, preferably, the metal auxiliary agent is selected from at least one of potassium nitrate, magnesium nitrate, zinc nitrate, chromium nitrate, cerium nitrate and zirconium nitrate.

[0023] On the other hand, the present invention also provides a desulfurizer prepared by any of the above-mentioned preparation methods. Preferably, the desulfurizer has a sulfur capacity of more than 30%, a porosity of more than 0.70%, and a pore volume of more than 0.70 mL / g; wherein the test method for sulfur capacity is carried out in accordance with the industry standard HG / T4354-2012.

[0024] The invention does not use expensive auxiliary agents, thus saving the production cost of the desulfurizer. The desulfurizer prepared by the invention is easy to shape, has a large porosity and pore volume, and has a high sulfur capacity, and can be regenerated for multiple times, thus having a good industrial application prospect. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0026] The "porosity" mentioned in the present invention refers to the percentage of the pore volume in the bulk material to the total volume of the material in its natural state.

[0027] The "pore volume" mentioned in the present invention, also known as pore volume, refers to the total volume of pores per unit mass of porous solids, and the unit is mL / g.

[0028] The "sulfur capacity" mentioned in the present invention is the working sulfur capacity, which refers to the mass of sulfur dioxide that can be absorbed by a unit mass of the desulfurizer under specified process conditions and is expressed as a percentage.

[0029] <Method for preparing desulfurizing agent>

[0030] The present invention uses iron-based raw materials to prepare active iron oxide, uses soluble ferrous salts and alkali to prepare hydroxy iron oxide seeds under appropriate reaction conditions, and uses the active iron oxide and the hydroxy iron oxide seeds as main active ingredients of the desulfurizer. By adding specific structural additives and suitable binders and metal additives, a desulfurizer with higher desulfurization ability is obtained while reducing production costs.

[0031] The method for preparing the desulfurizing agent of the present invention comprises the steps of preparing active iron oxide, preparing iron oxyhydroxide seed crystals and preparing the desulfurizing agent, which are described in detail below.

[0032] Preparation steps of activated iron oxide

[0033] Alkali is added to the iron-based raw material for neutralization reaction to form iron hydroxide, and the iron hydroxide is precipitated and dried to obtain active iron oxide.

[0034] The neutralization reaction of the present invention can be carried out at 100 to 150°C, preferably 110 to 140°C, and more preferably 120 to 130°C.

[0035] According to an embodiment of the present invention, an oxidizing atmosphere is blown into the neutralization reaction in step 1). The oxidizing atmosphere can be air, oxygen-containing inert gas or other oxygen-containing gas, preferably air.

[0036] In the present invention, the iron-based raw material can be any iron-containing material that can react with alkali to generate iron hydroxide, preferably an iron-containing industrial waste liquid, more preferably an acid leaching liquid of steelmaking converter mud. The present invention makes full use of recycled waste raw materials, reduces production costs and is also beneficial to environmental protection.

[0037] According to another embodiment of the present invention, the base in step 1) can be selected from at least one of aqueous ammonia, sodium hydroxide, sodium carbonate and sodium bicarbonate, preferably aqueous ammonia or sodium hydroxide, more preferably aqueous ammonia.

[0038] The concentration and dosage of ammonia water are determined according to the iron content of the iron-based raw material and the endpoint of the neutralization reaction, and the present invention is not particularly limited. According to one embodiment of the present invention, the mass concentration of ammonia water can be 5-28%, preferably 10-26%, and more preferably 20-25%. In order to save production costs, the neutralization reaction endpoint of the present invention is preferably a pH value of 7-8 in the system. Based on this, the volume ratio of the acid leaching solution and ammonia water can be 1:1-1:5, preferably 1:1.5-1:3, and more preferably 1:1.5-1:2.5. Reasonable ammonia concentration and dosage can save costs and shorten the time of neutralization reaction.

[0039] According to another embodiment of the present invention, the precipitation of the present invention is preferably natural precipitation. The drying temperature can be 80-120°C, preferably 85-115°C, more preferably 90-110°C; the drying time can be 1-20h, preferably 2-15h, more preferably 5-10h.

[0040] The method for preparing active iron oxide of the present invention has a simple process. When the prepared active iron oxide is used in a desulfurizer, the production cost is saved while the water resistance and strength of the desulfurizer are improved, which is beneficial to the molding of the desulfurizer.

[0041] Steps for preparing iron oxyhydroxide seed crystals

[0042] The mixed solution of the soluble ferrous salt and the precipitant is stirred and then aged to obtain a reaction product, and the reaction product is separated into a solid and a liquid to obtain ferric oxyhydroxide seed crystals.

[0043] According to one embodiment of the present invention, the molar ratio of ferrous ions to hydroxide ions in the mixed solution may be 1:0.7 to 1:1.5, preferably 1:0.9 to 1:1.3, and more preferably 1:1 to 1:1.2. The pH value of the mixed solution may be 7 to 9, preferably 7.5 to 8.7; more preferably 8.3 to 8.6. The molar ratio range of ferrous ions to hydroxide ions and the pH range in the mixed solution of the present invention are conducive to improving the pore volume and porosity of the iron oxyhydroxide seed crystals.

[0044] According to another embodiment of the present invention, the aging temperature can be 20-40°C, preferably 25-35°C, and more preferably 28-32°C; the aging time can be 2-10 hours, preferably 4-8 hours, and more preferably 5-7 hours. Reasonable aging temperature and time are conducive to the formation of iron oxyhydroxide seed crystals and increase the pore volume and porosity of the iron oxyhydroxide seed crystals.

[0045] In the present invention, the mixed solution can be stirred at a speed of 100 to 500 r / min, preferably 150 to 300 r / min, and more preferably 170 to 250 r / min. The stirring time can be 40 to 80 min, preferably 50 to 70 min; more preferably 55 to 65 min. Reasonable stirring conditions are conducive to improving the pore volume and porosity of the iron oxyhydroxide seed crystals.

[0046] According to one embodiment of the present invention, in step 2), the soluble ferrous salt may be selected from at least one of ferrous sulfate, ferrous chloride, ferrous nitrate and ferrous acetate; preferably, the soluble ferrous salt is selected from at least one of ferrous sulfate, ferrous chloride and ferrous nitrate; more preferably, the soluble ferrous salt is selected from at least one of ferrous sulfate and ferrous chloride.

[0047] According to another embodiment of the present invention, the precipitant can be selected from at least one of ammonia water, sodium hydroxide, calcium hydroxide, and sodium carbonate; preferably, the precipitant is selected from at least one of ammonia water, sodium hydroxide, and calcium hydroxide; more preferably, the precipitant is selected from at least one of sodium hydroxide and calcium hydroxide.

[0048] Reasonable soluble ferrous salt and precipitant are beneficial to the formation of ferric oxyhydroxide seeds and improve the pore volume and porosity of ferric oxyhydroxide seeds.

[0049] In the present invention, the solid-liquid separation method can use any filtration method known in the art, which is not particularly limited here, for example, it can be gravity filtration, pressure filtration, centrifugal filtration, vacuum filtration, etc. Various filtration methods can be implemented using equipment known in the art.

[0050] In the present invention, the reaction product is filtered and then washed, and the solid reaction product obtained is the iron oxyhydroxide seed crystal. The iron oxyhydroxide seed crystal prepared in the present invention is selected from at least one of α-FeOOH, β-FeOOH, γ-FeOOH, δ-FeOOH and amorphous FeOOH.

[0051] Preparation steps of desulfurization agent

[0052] Active iron oxide, iron oxyhydroxide seed crystals, a binder, a structural additive and a metal additive are mixed, formed, dried and roasted to obtain a desulfurizer.

[0053] According to one embodiment of the present invention, the calcination temperature can be 300-550°C, preferably 310-450°C, more preferably 320-380°C; the calcination time can be 1-8h, preferably 2-6h, more preferably 3-5h. Reasonable calcination temperature and time are conducive to the formation of the desulfurizer and increase the pore volume and porosity of the desulfurizer.

[0054] According to another embodiment of the present invention, the drying temperature can be 80-120°C, preferably 85-115°C, more preferably 90-110°C; the drying time can be 1-20h, preferably 2-15h, more preferably 5-10h. Reasonable drying temperature and time are helpful to maintain the internal structure of the desulfurizer and improve the pore volume and porosity of the desulfurizer.

[0055] In the present invention, the oxidizing atmosphere may be air, oxygen-containing inert gas or other oxygen-containing gas, preferably air.

[0056] The molding method can be any molding method known in the art, which is not particularly limited here, for example, mechanical rolling molding, mechanical pressing molding, extrusion molding, spiral extrusion molding, etc. Various molding methods can be implemented using equipment known in the art.

[0057] In the present invention, in parts by weight, the sum of the activated iron oxide and the ferric oxyhydroxide seed crystals may be 42 to 86.5 parts by weight, the binder may be 3 to 26 parts by weight, the structural additive may be 8.5 to 24 parts by weight, and the metal additive may be 2 to 8 parts by weight; preferably, the sum of the activated iron oxide and the ferric oxyhydroxide seed crystals is 60 to 84 parts by weight, the binder is 4 to 18 parts by weight, the structural additive is 9 to 15 parts by weight, and the metal additive is 3 to 7 parts by weight; more preferably, the sum of the activated iron oxide and the ferric oxyhydroxide seed crystals is 68 to 79 parts by weight, the binder is 7 to 14 parts by weight, the structural additive may be 10 to 12 parts by weight, and the metal additive may be 4 to 6 parts by weight.

[0058] According to one embodiment of the present invention, the weight ratio of active iron oxide to iron oxyhydroxide seed crystals can be 1:1 to 1:5, preferably 1:1 to 1:3, and more preferably 1:1 to 1:2. The ratio of iron oxide to iron oxyhydroxide seed crystals of the present invention can reduce production costs while ensuring that the desulfurizer has a higher sulfur capacity.

[0059] According to another embodiment of the present invention, the binder can be selected from at least one of gypsum, lime, calcium silicate, cement, and polyvinyl alcohol; preferably, the binder is selected from at least one of gypsum, lime, calcium silicate, and polyvinyl alcohol; more preferably, the binder is selected from at least one of lime, calcium silicate, and polyvinyl alcohol. A reasonable binder not only ensures the molding and strength of the desulfurizer, but also ensures that the desulfurizer has a higher pore volume and porosity.

[0060] In the present invention, the structural additives may include, by weight, 4 to 8 parts by weight of diatomaceous earth, 2.5 to 5 parts by weight of ammonium bicarbonate, and 2 to 6 parts by weight of polystyrene microspheres; preferably, the structural additives include 4 to 6 parts by weight of diatomaceous earth, 3 to 5 parts by weight of ammonium bicarbonate, and 3 to 5 parts by weight of polystyrene microspheres; more preferably, the structural additives include 4 to 5 parts by weight of diatomaceous earth, 3 to 4 parts by weight of ammonium bicarbonate, and 3 to 4 parts by weight of polystyrene microspheres.

[0061] The structural auxiliary agent of the present invention may also include at least one of bentonite and urea.

[0062] Reasonable structural additives can improve the water resistance and specific surface area of ​​the desulfurizer, and help to increase the pore volume and porosity of the desulfurizer.

[0063] According to one embodiment of the present invention, the metal additive can be selected from at least one of alkali metal salts, alkaline earth metal salts and transition metal salts; preferably, the metal additive is selected from at least one of potassium nitrate, magnesium nitrate, zinc nitrate, chromium nitrate, cerium nitrate and zirconium nitrate; more preferably, the metal additive is selected from at least one of potassium nitrate, magnesium nitrate, zinc nitrate and chromium nitrate. The metal additive added in the present invention is conducive to improving the water resistance and anti-poisoning of the desulfurizer, and promotes the formation of a dispersed three-dimensional pore structure, thereby increasing the pore volume and porosity of the desulfurizer.

[0064] <Desulfurization agent>

[0065] The desulfurizing agent of the present invention can be obtained by adopting the above method.

[0066] The desulfurizer of the present invention has high iron oxide content, excellent strength and water resistance, large porosity and pore volume, high sulfur capacity and strong desulfurization ability. The sulfur capacity of the desulfurizer can reach more than 30%, the porosity can reach more than 0.70%, and the pore volume can reach more than 0.70mL / g.

[0067] According to one embodiment of the present invention, the test method of sulfur capacity is carried out in accordance with the industry standard HG / T4354-2012.

[0068] According to another embodiment of the present invention, the use conditions of the desulfurizer are as follows:

[0069] Applicable temperature: 20~60℃; air speed: 500~1500h -1 ; Empty tower linear velocity: 0.10~0.30m / s; Pressure: normal pressure (0.1MPa)~8MPa; Humidity: close to saturated water vapor.

[0070] <Ingredients>

[0071] Unless otherwise specified, the raw materials used in the following examples are all commercially available products.

[0072] <Test Method>

[0073] The pore volume and porosity of the material in the present invention were measured using the American ASAP 2460 fully automatic rapid physical adsorption analyzer based on the working principle of the isothermal physical adsorption static capacity method.

[0074] The sulfur capacity test of the material in the present invention was carried out with reference to the method in the industry standard HG / T4354-2012 "Sulfur capacity test method for iron oxide desulfurizer at room temperature".

[0075] Example 1 and Comparative Examples 1 to 3

[0076] 1. Preparation of activated iron oxide:

[0077] The acid leaching liquid of steelmaking converter mud recycled from steel plants is used as iron-based raw material.

[0078] Air is blown into the acid leaching liquid of the steelmaking converter mud while continuously adding a 24% ammonia solution by mass to carry out a neutralization reaction at 120°C. When the pH value in the reaction system reaches 7.5, the addition of ammonia solution is stopped and the generated iron hydroxide is naturally precipitated.

[0079] The precipitated iron hydroxide was taken out and dried at 100°C for 8 hours to obtain active iron oxide.

[0080] 2. Preparation of iron oxyhydroxide seed crystals:

[0081] 34 parts by weight of ferrous sulfate and 20 parts by weight of ferrous chloride are mixed and water is added to prepare a soluble ferrous salt solution; 15 parts by weight of sodium hydroxide and 5 parts by weight of calcium hydroxide are mixed and water is added to prepare an alkaline solution.

[0082] According to the molar ratio of ferrous ion to hydroxide ion of 1:1, the soluble ferrous salt solution and the alkaline solution were mixed and stirred at 250r / min for 60min. Then, the mixture was aged at 30°C for 6h to obtain a reaction product, which was filtered under pressure and washed with water three times to obtain a brown-yellow filter cake to obtain iron oxyhydroxide seed crystals.

[0083] 3. Prepare desulfurizers according to the formula in Table 1:

[0084] The prepared active iron oxide and iron oxyhydroxide seed crystals are mixed evenly with lime, calcium silicate, polyvinyl alcohol, diatomaceous earth, ammonium bicarbonate, polystyrene microspheres, potassium nitrate, magnesium nitrate, zinc nitrate and chromium nitrate, and extruded into strips using a screw extruder. The strips are placed in hot air and dried. The dried strips are roasted and cooled to obtain a desulfurizer.

[0085] A desulfurization experiment was conducted on the blast furnace flue gas collected from a steel plant in a fixed bed adsorption tower using the desulfurizer prepared in Example 1 and Comparative Examples 1 to 3.

[0086] The total sulfur content in blast furnace flue gas is 180 mg / m 3 , of which carbonyl sulfide and carbon disulfide account for 65wt% of the total sulfur content, and hydrogen sulfide accounts for 25wt% of the total sulfur content.

[0087] Desulfurization temperature: 40℃; air velocity: 1000h -1 ; Empty tower linear velocity: 0.2m / s; Pressure: 2MPa; Humidity: saturated.

[0088] The performance data of the desulfurizers prepared in the above Example 1 and Comparative Examples 1 to 3 are shown in Table 1.

[0089] Table 1

[0090]

[0091]

[0092] It can be seen from Table 1 that the desulfurizer prepared by the present invention has a larger porosity and pore volume, a higher sulfur capacity, and a strong desulfurization ability.

[0093] It can also be seen from Table 1 that the ratio of structural additives is crucial to the desulfurization performance of the desulfurizer. Lack of ammonium bicarbonate or polystyrene microspheres will lead to a decrease in the pore volume and porosity of the desulfurizer and a decrease in sulfur capacity. Reducing the amount of diatomaceous earth and ammonium bicarbonate will also lead to a decrease in the pore volume and porosity of the desulfurizer and a decrease in sulfur capacity.

[0094] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a desulfurizing agent, comprising the following steps: 1) Preparation of activated iron oxide: adding alkali to an iron-based raw material, performing a neutralization reaction at 100-150° C. to form iron hydroxide, and drying the iron hydroxide precipitate to obtain activated iron oxide; 2) preparing ferric oxyhydroxide seed crystals: stirring a mixed solution of a soluble ferrous salt and a precipitant, aging the solution to obtain a reaction product, and separating the reaction product into a solid and liquid to obtain ferric oxyhydroxide seed crystals; wherein the molar ratio of ferrous ions to hydroxide ions in the mixed solution is 1:0.7 to 1:1.5; 3) Mixing active iron oxide, iron oxyhydroxide seed crystals, a binder, a structural additive and a metal additive, drying, and calcining at 300-550° C. for 1-8 hours to obtain a desulfurizer; wherein the structural additive comprises, by weight, 4-8 parts by weight of diatomaceous earth, 2.5-5 parts by weight of ammonium bicarbonate, and 2-6 parts by weight of polystyrene microspheres.

2. The preparation method according to claim 1, characterized in that: An oxidizing atmosphere is blown into the neutralization reaction.

3. The preparation method according to claim 1 or 2, characterized in that: The alkali in step 1) is selected from at least one of aqueous ammonia, sodium hydroxide, sodium carbonate and sodium bicarbonate.

4. The preparation method according to claim 1, characterized in that: In step 2), the pH value of the mixed solution is 7 to 9, the aging temperature is 20 to 40° C., and the aging time is 2 to 10 hours.

5. The preparation method according to claim 1 or 4, characterized in that: In step 2), the soluble ferrous salt is selected from at least one of ferrous sulfate, ferrous chloride, ferrous nitrate and ferrous acetate; The precipitant is selected from at least one of ammonia water, sodium hydroxide, calcium hydroxide and sodium carbonate.

6. The preparation method according to claim 1, characterized in that: The drying in step 3) is carried out in an oxidizing atmosphere, the drying temperature is 80 to 120° C., and the drying time is 1 to 20 hours.

7. The preparation method according to claim 1 or 6, characterized in that: In step 3), the sum of the weights of the activated iron oxide and the hydroxy iron oxyhydroxide seed crystals is 42 to 86.5 parts by weight, the binder is 3 to 26 parts by weight, the structural additive is 8.5 to 24 parts by weight, and the metal additive is 2 to 8 parts by weight, wherein the weight ratio of the activated iron oxide to the hydroxy iron oxyhydroxide seed crystals is 1:1 to 1:

5.

8. The preparation method according to claim 7, characterized in that: The binder is selected from at least one of gypsum, lime, calcium silicate, cement and polyvinyl alcohol; The metal additive is selected from at least one of an alkali metal salt, an alkaline earth metal salt and a transition metal salt; The structural auxiliary agent also includes at least one of bentonite and urea.

9. The preparation method according to claim 8, characterized in that: The metal additive is selected from at least one of potassium nitrate, magnesium nitrate, zinc nitrate, chromium nitrate, cerium nitrate and zirconium nitrate.

10. A desulfurizing agent obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The sulfur capacity of the desulfurizer is above 30%, the porosity is above 0.70%, and the pore volume is above 0.70 mL / g; wherein the test method of the sulfur capacity is carried out in accordance with the industry standard HG / T4354-2012.

Citation Information

Cited By

  • Reusable iron oxyhydroxide desulfurizer and preparation method thereof

    CN121668937A