Rare earth oxide-noble metal catalyst for hydrogen isotope oxidation as well as preparation method and application of rare earth oxide-noble metal catalyst

Through the preparation method of rare earth oxide-precious metal catalyst, the problems of low catalyst activity and poor stability are solved, and the efficient performance of low-temperature hydrogen isotope oxidation reaction and long-term recycling are achieved, reducing costs.

CN119034792APending Publication Date: 2024-11-29MATERIAL INST OF CHINA ACADEMY OF ENG PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411152730.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing catalysts for hydrogen isotope exhaust gas oxidation are low and have poor stability, resulting in a degradation of the catalyst's performance at high temperatures and sintering and agglomeration.

Method used

Using the preparation method of rare earth oxide-precious metal catalyst, the catalyst precursor is prepared by complexing precious metal salts with organic ligands, rare earth metal salts with organic ligands, combined with silicon source and template agents to carry out hydrothermal reactions, and then calcination is performed. and the reduction step form rare earth oxide-noble metal clusters bounded in the pure silicon molecular sieve structure to avoid agglomeration.

Benefits of technology

The temperature required for hydrogen isotope oxidation reaction is reduced, the oxidation reaction performance of the catalyst is improved, and the stability is enhanced. The content of precious metals and rare earth oxides is smaller and the cost is lower, and the performance of the catalyst is not attenuated during continuous recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034792A_ABST
    Figure CN119034792A_ABST
Patent Text Reader

Abstract

The invention provides a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation as well as a preparation method and application of the rare earth oxide-noble metal catalyst. The preparation method of the rare earth oxide-noble metal catalyst for hydrogen isotope oxidation comprises the following steps: mixing noble metal salt with an organic ligand to obtain a noble metal complex solution; mixing a rare earth metal salt with an organic ligand to obtain a rare earth metal complex solution; mixing a silicon source, a template agent, deionized water, the noble metal complex solution and the rare earth metal complex solution to obtain a precursor solution; performing hydrothermal reaction on the precursor solution to obtain a catalyst precursor; and cleaning the catalyst precursor, drying, calcining, and reducing to obtain the rare earth oxide-noble metal catalyst. According to the rare earth oxide-noble metal catalyst prepared by the preparation method disclosed by the invention, the oxidation reaction performance of the catalyst is jointly improved due to the unique electronic structure of the rare earth metal oxide and the noble metal serving as an oxygen source, and the temperature required by a hydrogen isotope oxidation reaction is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of hydrogen isotope waste gas treatment catalysts, in particular to a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation and a preparation method and application thereof. Background Art

[0002] When a fusion experiment device or a fusion reactor is in operation, hydrogen isotope gas, especially radioactive tritium, used as fuel is usually discharged into the air due to permeation or leakage, causing harm to the environment and public health. Therefore, it is necessary to find a method to efficiently and safely remove the waste gas containing hydrogen isotopes.

[0003] The catalytic oxidation technology of hydrogen isotopes is considered as one of the effective means to treat tritium-containing waste gas. By catalytic oxidation, tritium gas is converted into tritium water for collection, thereby reducing its harm to the environment and the public. Existing noble metal catalysts often have problems such as low catalyst activity and poor catalyst stability in the catalytic oxidation process of tritium gas. Summary of the invention

[0004] The present invention aims to solve the problems of low activity (for example, the temperature required for the oxidation reaction is relatively high, usually greater than 100°C) and poor stability (for example, sintering and agglomeration of precious metal particles in the catalyst, resulting in performance degradation after long-term or repeated use) of existing hydrogen isotope waste gas oxidation reaction catalysts, and proposes a rare earth oxide-precious metal catalyst for hydrogen isotope oxidation and a preparation method and application thereof.

[0005] The technical method of the present invention is as follows:

[0006] The present invention provides a method for preparing a rare earth oxide-noble metal catalyst, the preparation method comprising:

[0007] mixing a noble metal salt with an organic ligand to obtain a noble metal complex solution;

[0008] Mixing a rare earth metal salt with an organic ligand to obtain a rare earth metal complex solution;

[0009] Mixing a silicon source, a template, deionized water, a noble metal complex solution, and a rare earth metal complex solution to obtain a precursor solution;

[0010] subjecting the precursor solution to a hydrothermal reaction to obtain a catalyst precursor;

[0011] The catalyst precursor is washed and dried, and then calcined and reduced to obtain a rare earth oxide-noble metal catalyst.

[0012] The precious metal salt includes platinum salt and / or palladium salt, the platinum salt includes one or more of platinum dichloride, chloroplatinic acid, sodium chloroplatinate, the palladium salt includes palladium dichloride and / or sodium chloropalladate; the rare earth metal salt includes one or more of lanthanum nitrate, cerium nitrate, praseodymium nitrate and neodymium nitrate.

[0013] The organic ligand includes any one of ethylenediamine, dimethyldiethylamine, diethylenetriamine and acetylacetone.

[0014] The silicon source includes one or more of tetraethoxysilane, methyltriethoxysilane, methyltripropoxysilane and trimethoxysilane.

[0015] The template agent is any one of tetrapropylammonium hydroxide, tetrapropylammonium bromide and n-butylamine.

[0016] The molar ratio of the noble metal salt to the organic ligand is 1:16-28; the molar ratio of the rare earth metal salt to the organic ligand is 1:10-25.

[0017] The molar ratio of the silicon source, the template, the deionized water, the noble metal complex solution and the rare earth metal complex solution is 1: 0.2-0.66: 33.5-65.5: 0.002-0.018: 0.001-0.006.

[0018] Specifically, the temperature of the hydrothermal reaction of the precursor solution is 150-200° C.; the hydrothermal time is 24-96 hours.

[0019] Specifically, the steps of washing and drying the catalyst precursor include: washing the catalyst precursor with deionized water until it is neutral, and drying; wherein the drying temperature is 50-150° C.; and the drying time is 4-16 hours.

[0020] Specifically, the step of calcining the catalyst precursor includes: calcining the catalyst precursor in air; wherein the calcination temperature is 400-600° C., and the calcination time is 2-8 hours.

[0021] Specifically, the reduction step of the catalyst precursor includes: reducing the calcined product under a mixed atmosphere; wherein the reduction temperature is 300-500°C, the reduction time is 2-8h, the mixed atmosphere includes hydrogen and argon, and the volume ratio of hydrogen to argon is 0.5-1.0:9.5-9.0.

[0022] In the present invention, the method further comprises: the present invention provides a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation, and the catalyst is obtained by the preparation method of the rare earth oxide-noble metal catalyst mentioned above.

[0023] The active sites of the rare earth metal oxide and the noble metal of the catalyst are confined in the pure silicon molecular sieve structure, and the average particle size of the rare earth oxide-noble metal clusters is less than 4nm.

[0024] The present invention provides an application of the rare earth oxide-noble metal catalyst in hydrogen isotope catalytic oxidation.

[0025] The beneficial effects of the present invention are:

[0026] (1) The present invention prepares a rare earth oxide-noble metal catalyst by combining noble metals and rare earths. The rare earth metal oxide, due to its unique electronic structure, and the noble metal as an oxygen source, jointly improves the oxidation reaction performance of the catalyst and reduces the temperature required for the hydrogen isotope oxidation reaction (≤50°C).

[0027] (2) The catalyst of the present invention confines the active sites of rare earth metal oxides and precious metals in the pore structure of pure silicon molecular sieve. Due to the limiting effect of the pore structure, these active sites will not undergo obvious agglomeration during the heating process, thereby avoiding sintering and agglomeration, which would cause low activity and poor stability.

[0028] (3) The catalyst of the present invention confines the active sites of rare earth metal oxides and noble metals in the pore structure of pure silicon molecular sieve, thereby better controlling the particle size of rare earth oxide-noble metal clusters (average size <4 nm).

[0029] (4) In the catalyst of the present invention, the contents of precious metals and rare earth oxides are both ≤0.5wt.%, so the usage amount is small and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is the XRD spectrum of the catalyst of Example 1 of the present invention;

[0031] Figure 2 is the HAADF diagram of the catalyst of Example 1 of the present invention;

[0032] Figure 3 is a particle size distribution diagram of the catalyst of Example 1 of the present invention;

[0033] Figure 4 FT-IR image of the catalyst of Example 2 of the present invention;

[0034] Figure 5 TEM image of the catalyst of Example 3 of the present invention;

[0035] Figure 6 This is the EDS image of the catalyst of Example 3 of the present invention;

[0036] Figure 7This is a restart performance test diagram of the catalyst of Example 1 of the present invention for oxidizing hydrogen isotopes. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention provides a method for preparing a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation, the preparation method comprising:

[0039] S1. Mixing a noble metal salt with an organic ligand to obtain a noble metal complex solution.

[0040] In one embodiment, the noble metal salt includes a platinum salt and / or a palladium salt. The platinum salt includes one or more of platinum dichloride, chloroplatinic acid, and sodium chloroplatinate, and the palladium salt includes palladium dichloride and / or sodium chloropalladate.

[0041] In one embodiment, the molar ratio of the noble metal salt to the organic ligand is 1:16-28. For example, the molar ratio of the noble metal salt to the organic ligand is 1:18, 1:22, or 1:25.

[0042] In one embodiment, at room temperature, the noble metal salt and the organic ligand are mixed for 30-150 minutes, for example, for 50 minutes, 100 minutes, or 130 minutes.

[0043] In one embodiment, the present invention uses platinum and / or palladium because they have good hydrogen and hydrogen isotope gas cracking capabilities.

[0044] S2. Mixing the rare earth metal salt and the organic ligand to obtain a rare earth metal complex solution.

[0045] In one embodiment, the metal in the rare earth metal salt may be a light rare earth element, for example, the rare earth metal salt includes one or more of lanthanum nitrate, cerium nitrate, praseodymium nitrate and neodymium nitrate, which can significantly improve the catalyst performance.

[0046] In one embodiment, the molar ratio of the rare earth metal salt to the organic ligand is 1:10-25. For example, the molar ratio of the rare earth metal salt to the organic ligand is 1:15, 1:18, or 1:22.

[0047] In one embodiment, at room temperature, the rare earth metal salt and the organic ligand are mixed for 30-150 minutes, for example, for 50 minutes, 100 minutes, or 130 minutes.

[0048] Specifically, precious metals and rare earth metals are protected by complexing with organic ligands. If the precious metal salts and rare earth metal salts are directly mixed, the precious metals and rare earth metals will precipitate quickly due to the acidity and alkalinity of the reaction environment, making it impossible to prepare the catalyst.

[0049] S3, mixing the silicon source, the template, deionized water, the noble metal complex solution and the rare earth metal complex solution to obtain a precursor solution.

[0050] Specifically, the silicon source is the main component of the molecular sieve synthesis. The template is added to assist the synthesis of the molecular sieve. The deionized water is added because the catalyst is synthesized by hydrothermal reaction (in an aqueous solution environment). Here, the deionized water can also avoid interference from other ions in the synthesis of the catalyst.

[0051] In one embodiment, the molar ratio of the silicon source, the template, the deionized water, the noble metal complex solution, and the rare earth metal complex solution is 1: 0.2-0.66: 33.5-65.5: 0.002-0.018: 0.001-0.006.

[0052] The organic ligand includes any one of ethylenediamine, dimethyldiethylamine, diethylenetriamine and acetylacetone.

[0053] The silicon source includes one or more of tetraethoxysilane, methyltriethoxysilane, methyltripropoxysilane and trimethoxysilane.

[0054] Wherein, the template agent is any one of tetrapropylammonium hydroxide, tetrapropylammonium bromide and n-butylamine.

[0055] In one embodiment, the silicon source, template, deionized water, noble metal complex solution and rare earth metal complex solution are mixed for 2-15 hours, for example, for 3 hours, 8 hours or 10 hours.

[0056] S4. subjecting the precursor solution to a hydrothermal reaction to obtain a catalyst precursor.

[0057] In one embodiment, the hydrothermal temperature is 150-200° C. and the hydrothermal time is 24-96 hours. For example, the hydrothermal temperature is 160° C., 170° C., 190° C. and the hydrothermal time is 36 hours, 48 ​​hours, or 75 hours.

[0058] Specifically, during the hydrothermal process, the rare earth metal and the noble metal in the catalyst precursor exist in the form of a complex. During the subsequent calcination and reduction process, the catalyst precursor forms clusters of noble metal and rare earth oxide.

[0059] S5. Washing and drying the catalyst precursor, calcining and then reducing it to obtain a rare earth oxide-noble metal catalyst.

[0060] Specifically, the steps of washing and drying the catalyst precursor include: washing the catalyst precursor with deionized water until it is neutral, drying, and then calcining and reducing.

[0061] Here, washing is to remove some organic matter in the solution after the hydrothermal reaction. For example, washing can be performed by centrifugal washing. Drying is to obtain a powder catalyst.

[0062] The drying temperature is 50-150°C and the drying time is 4-16h. For example, the drying temperature is 60°C, 70°C, 90°C and the drying time is 5h, 10h, 12h.

[0063] In one embodiment, the calcination step includes: calcining the catalyst precursor in air, wherein the calcination temperature is 400-600° C., and the calcination time is 2-8 hours. For example, the calcination temperature is 450° C., 500° C., 550° C., and the calcination time is 4 hours, 6 hours, or 7 hours.

[0064] In one embodiment, the reduction step includes: reducing the calcined product in a mixed atmosphere, wherein the reduction temperature is 300-500° C., the reduction time is 2-8 hours, the mixed atmosphere includes hydrogen and argon, and the volume ratio of hydrogen to argon is 0.5-1.0:9.5-9.0. For example, the reduction temperature is 350° C., 400° C., 450° C., and the reduction time is 4 hours, 6 hours, or 7 hours.

[0065] Specifically, the catalyst after drying exists in the form of a complex, and at this time the catalyst has no catalytic activity. Therefore, it is necessary to remove the organic ligands that complex the precious metal and the rare earth metal through the calcination-reduction method, and finally obtain a catalyst with catalytic activity.

[0066] Specifically, if pure hydrogen is used, it will be dangerous under high temperature conditions. The use of mixed gases (for example, 10% H2 / Ar mixed gas) has been able to be used to reduce the precious metals in the catalyst. At the same time, the use of hydrogen can reduce the precious metals, making them active and able to crack hydrogen isotope gases.

[0067] Here, in the catalyst prepared by the preparation method of the present invention, since platinum metal has a good cracking ability for H2 (and hydrogen isotopes), rare earth metal oxides can be used as an oxygen source to promote catalytic oxidation.

[0068] The present invention provides a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation. The rare earth oxide-noble metal catalyst is obtained by the preparation method of the rare earth oxide-noble metal catalyst.

[0069] In the prior art, the existence state of the noble metal (active sites) in the noble metal catalyst, such as the noble metal on the surface of the catalyst carrier, will agglomerate when heated, resulting in a decrease in the number of active sites of the catalyst and a decrease in catalytic activity. However, the present invention restricts the noble metal and rare earth oxide in the pore structure of the molecular sieve material. Due to the restriction of the pore structure, these active sites will not significantly agglomerate during calcination and reduction.

[0070] In one embodiment, the active sites of the rare earth metal oxide and noble metal (eg, metal oxide and noble metal clusters) of the catalyst are confined in a pure silicon molecular sieve (composed of Si and O elements) structure, and the average particle size of the rare earth oxide-noble metal clusters is less than 4 nm.

[0071] The present invention provides an application of the rare earth oxide-noble metal catalyst in hydrogen isotope catalytic oxidation.

[0072] When the catalyst of the present invention is used for hydrogen isotope catalytic oxidation, the reaction temperature can be lower than 50°C.

[0073] Here, when the catalyst of the present invention is used for hydrogen isotope catalytic oxidation, the catalytic performance is not attenuated after continuous cycle operation for more than 7 times.

[0074] In order to better understand the above exemplary embodiments of the present invention, they are further described below with reference to specific examples.

[0075] Example 1

[0076] Step 1: Platinum dichloride and organic ligand ethylenediamine are mixed at a molar ratio of 1:20, and the solution is stirred on a magnetic stirrer at room temperature for 60 minutes to obtain a platinum complex solution.

[0077] Step 2: Mix lanthanum nitrate salt and organic ligand acetylacetone at a molar ratio of 1:20, place the solution on a magnetic stirrer and stir at room temperature for 60 minutes to obtain a lanthanum complex solution.

[0078] Step 3: Prepare a solution with a molar ratio of silicon source tetraethoxysilane, template agent tetrapropylammonium hydroxide, deionized water, platinum complex solution and lanthanum complex solution of 1:0.4:35:0.0023:0.002, and fully mix and stir at room temperature for 5 hours to obtain a precursor solution.

[0079] Step 4: Place the precursor solution obtained in step 3 in a polytetrafluoroethylene liner and place it in a reactor. After reacting for 72 hours at a constant temperature of 170°C in a drying oven, wash the material obtained after the reaction with deionized water until it is neutral, and dry it in a drying oven at 80°C for 4 hours to obtain a dry powder material.

[0080] Step 5: The powder material is first calcined at 550° C. for 6 h, and then reduced at 400° C. for 2 h in a 10% hydrogen-argon mixed atmosphere to obtain a catalyst.

[0081] The catalyst contains 0.52 wt.% of platinum and 0.15 wt.% of lanthanum. Figure 1 It is the physical result of the catalyst. Figure 2 and Figure 3 The average particle size of the lanthanum oxide-platinum clusters in the catalyst is 2.9 nm.

[0082] Example 2

[0083] Step 1: Platinum dichloride and organic ligand ethylenediamine are mixed at a molar ratio of 1:20, and the solution is stirred on a magnetic stirrer at room temperature for 60 minutes to obtain a platinum complex solution.

[0084] Step 2: Mix cerium nitrate salt and organic ligand ethylenediamine at a molar ratio of 1:20, place the solution on a magnetic stirrer and stir at room temperature for 60 minutes to obtain a cerium complex solution.

[0085] Step 3: Prepare a solution with a molar ratio of silicon source tetraethoxysilane, template agent tetrapropylammonium hydroxide, deionized water, platinum complex solution and cerium complex solution of 1:0.4:35:0.0023:0.002, and fully mix and stir at room temperature for 5 hours to obtain a precursor solution.

[0086] Step 4: Place the precursor solution obtained in step 3 in a polytetrafluoroethylene liner and place it in a reactor. After reacting for 72 hours at a constant temperature of 170°C in a drying oven, wash the material obtained by the reaction with deionized water until it is neutral, and dry it in a drying oven at 80°C for 4 hours to obtain a dry powder material.

[0087] Step 5: The powder material is first calcined at 550° C. for 6 h, and then reduced at 400° C. for 2 h in a 10% hydrogen-argon mixed atmosphere to obtain a catalyst.

[0088] In the catalyst, the content of platinum is 0.53 wt.%, and the content of cerium is 0.17 wt.%. Figure 4 Here, the average particle size of the cerium oxide-platinum clusters in the catalyst is 2.9 nm.

[0089] Example 3

[0090] Step 1: Platinum dichloride and organic ligand ethylenediamine are mixed at a molar ratio of 1:20, and the solution is stirred on a magnetic stirrer at room temperature for 60 minutes to obtain a platinum complex solution.

[0091] Step 2: Mix the rare earth metal salt praseodymium nitrate and the organic ligand ethylenediamine at a molar ratio of 1:20, place the solution on a magnetic stirrer and stir at room temperature for 60 minutes to obtain a praseodymium complex solution.

[0092] Step 3: Prepare a solution with a molar ratio of silicon source tetraethoxysilane, template agent tetrapropylammonium hydroxide, deionized water, platinum complex solution and praseodymium complex solution of 1:0.4:35:0.0023:0.002, and fully mix and stir at room temperature for 5 hours to obtain a precursor solution.

[0093] Step 4: Place the precursor solution obtained in step 3 in a polytetrafluoroethylene liner and place it in a reactor. After reacting for 72 hours at a constant temperature of 170°C in a drying oven, wash the material obtained after the reaction with deionized water until it is neutral, and dry it in a drying oven at 80°C for 4 hours to obtain a dry powder material.

[0094] Step 5: The powder material is first calcined at 550° C. for 6 h, and then reduced at 400° C. for 2 h in a 10% hydrogen-argon mixed atmosphere to obtain a catalyst.

[0095] The content of platinum in the catalyst is 0.51wt.%, and the content of praseodymium is 0.16wt.%. The TEM-ESD results of the obtained catalyst are as follows: Figure 5 and Figure 6 Here, the average particle size of the praseodymium oxide-platinum clusters in the catalyst is about 3.2 nm.

[0096] Example 4

[0097] Step 1: palladium dichloride and organic ligand ethylenediamine are mixed at a molar ratio of 1:20, and the solution is stirred on a magnetic stirrer at room temperature for 60 minutes to obtain a palladium complex solution.

[0098] Step 2: Mix the rare earth metal salt lanthanum nitrate and the organic ligand ethylenediamine at a molar ratio of 1:20, place the solution on a magnetic stirrer and stir at room temperature for 60 minutes to obtain a lanthanum complex solution.

[0099] Step 3: Prepare a solution with a molar ratio of silicon source tetraethoxysilane, template agent tetrapropylammonium hydroxide, deionized water, palladium complex solution and lanthanum complex solution of 1:0.4:35:0.0023:0.002, and fully mix and stir at room temperature for 5 hours to obtain a precursor solution.

[0100] Step 4: Place the precursor solution obtained in step 3 in a polytetrafluoroethylene liner and place it in a reactor. After reacting for 72 hours at a constant temperature of 170°C in a drying oven, wash the material obtained after the reaction with deionized water until it is neutral, and dry it in a drying oven at 80°C for 4 hours to obtain a dry powder material.

[0101] Step 5: The powder material is first calcined at 550° C. for 6 h, and then reduced at 400° C. for 2 h in a 10% hydrogen-argon mixed atmosphere to obtain a catalyst.

[0102] The content of palladium in the catalyst is 0.55 wt.%, and the content of lanthanum is 0.13 wt.%. Here, the average particle size of the lanthanum oxide-palladium clusters in the catalyst is about 3.1 nm.

[0103] Evaluation of Catalyst Performance for Catalytic Oxidative Removal of Hydrogen Isotopes

[0104] Evaluation of the hydrogen isotope removal reaction performance of Example 1

[0105] 50 mg of the catalyst material of Example 1 was placed in a reaction tube, and a hydrogen-oxygen (or deuterium-oxygen) mixed gas with a hydrogen concentration of 2000 ppm was introduced at a reaction temperature of 40° C., and the space velocity was controlled to be 24000 mL·g -1 ·h -1 The reaction time was 200 min. The tail gas of the reaction was detected by a tail end chromatography device, and the hydrogen conversion rate of the catalyst is shown in Table 1.

[0106] Evaluation of the Hydrogen Isotope Reaction Performance of Example 2

[0107] 50 mg of the catalyst material of Example 2 was placed in a reaction tube, and a hydrogen-oxygen (or deuterium-oxygen) mixed gas with a hydrogen concentration of 2000 ppm was introduced at a reaction temperature of 50° C., and the space velocity was controlled to be 48000 mL·g -1 ·h -1 The reaction time was 200 min. The tail gas of the reaction was detected by a tail end chromatography device, and the hydrogen conversion rate of the catalyst is shown in Table 1.

[0108] Evaluation of the Hydrogen Isotope Reaction Performance of Example 3

[0109] 50 mg of catalyst material was placed in a reaction tube, and a hydrogen-oxygen (or deuterium-oxygen) mixed gas with a hydrogen concentration of 2000 ppm was introduced at a reaction temperature of 40°C, and the space velocity was controlled to be 48000 mL·g -1 ·h -1 The reaction time was 200 min. The tail gas of the reaction was detected by a tail end chromatography device, and the hydrogen conversion rate of the catalyst is shown in Table 1.

[0110] Evaluation of the Hydrogen Isotope Reaction Performance of Example 4

[0111] 50 mg of the catalyst material of Example 1 was placed in a reaction tube, and a hydrogen-oxygen (or deuterium-oxygen) mixed gas with a hydrogen concentration of 2000 ppm was introduced at a reaction temperature of 50° C., and the space velocity was controlled to be 24000 mL·g-1 ·h -1 The reaction time was 200 min. The tail gas of the reaction was detected by a tail end chromatography device, and the hydrogen conversion rate of the catalyst is shown in Table 1.

[0112] At the same time, the catalyst restart performance was tested. The experimental test conditions were consistent with the dehydrogenation reaction performance evaluation of Example 1. The total reaction time of the cyclic application test was 93900 min. The reaction tail gas was detected by the tail end chromatography device. The hydrogen conversion rate of the catalyst is shown in Figure 7 .

[0113] Catalyst samples Example 1 Example 2 Example 3 Example 4 Hydrogen conversion rate (%) 99.3 99.9 98.6 96.1 Deuterium conversion rate (%) 98.5 98.8 97.5 95.2

[0114] Table 1

[0115] It should be noted that the present invention can use hydrogen and deuterium instead of tritium to verify the catalytic oxidation conversion rate, and can also use tritium to verify the catalytic oxidation conversion rate.

[0116] It can be seen from Table 1 that the hydrogen and hydrogen isotope conversion rates in Examples 1-4 are all above 90%, and the reaction temperatures are all below 50°C.

[0117] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a rare earth oxide-noble metal catalyst for hydrogen isotope oxidation, characterized in that: The preparation method comprises: mixing a noble metal salt with an organic ligand to obtain a noble metal complex solution; mixing a rare earth metal salt with an organic ligand to obtain a rare earth metal complex solution; Mixing a silicon source, a template, deionized water, a noble metal complex solution, and a rare earth metal complex solution to obtain a precursor solution; subjecting the precursor solution to a hydrothermal reaction to obtain a catalyst precursor; The catalyst precursor is washed and dried, calcined and then reduced to obtain a rare earth oxide-noble metal catalyst.

2. The preparation method according to claim 1, characterized in that The temperature of the hydrothermal reaction of the precursor solution is 150-200° C.; the hydrothermal time is 24-96 hours.

3. The preparation method according to claim 1, characterized in that The steps of washing and drying the catalyst precursor include: The catalyst precursor is washed with deionized water until neutral and dried; wherein the drying temperature is 50-150° C. and the drying time is 4-16 hours.

4. The preparation method according to claim 1, characterized in that The steps of calcining the catalyst precursor include: The catalyst precursor is calcined in air; wherein the calcination temperature is 400-600° C. and the calcination time is 2-8 hours.

5. The preparation method according to claim 3, characterized in that The steps of reducing the catalyst precursor include: The calcined product is reduced in a mixed atmosphere; wherein the reduction temperature is 300-500° C., the reduction time is 2-8 hours, the mixed atmosphere comprises hydrogen and argon, and the volume ratio of hydrogen to argon is 0.5-1.0:9.5-9.

0.

6. The preparation method according to claim 1, characterized in that The precious metal salts include platinum salts and / or palladium salts, the platinum salts include one or more of platinum dichloride, chloroplatinic acid, and sodium chloroplatinate, and the palladium salts include palladium dichloride and / or sodium chloropalladate; the rare earth metal salts include one or more of lanthanum nitrate, cerium nitrate, praseodymium nitrate, and neodymium nitrate.

7. The preparation method according to claim 1, characterized in that The organic ligand includes any one of ethylenediamine, dimethyldiethylamine, diethylenetriamine, and acetylacetone.

8. The preparation method according to claim 1, characterized in that The silicon source includes one or more of tetraethoxysilane, methyltriethoxysilane, methyltripropoxysilane, and trimethoxysilane.

9. The preparation method according to claim 1, characterized in that The template agent is any one of tetrapropylammonium hydroxide, tetrapropylammonium bromide and n-butylamine.

10. The preparation method according to claim 1, characterized in that The molar ratio of the noble metal salt to the organic ligand is 1:16-28; the molar ratio of the rare earth metal salt to the organic ligand is 1:10-25.

11. The preparation method according to claim 1, characterized in that The molar ratio of the silicon source, the template, the deionized water, the noble metal complex solution and the rare earth metal complex solution is 1:0.2-0.66:33.5-65.5:0.002-0.018:0.001-0.

006.

12. A rare earth oxide-noble metal catalyst for hydrogen isotope oxidation, characterized in that: The rare earth oxide-noble metal catalyst is obtained by the preparation method of the rare earth oxide-noble metal catalyst for hydrogen isotope oxidation according to any one of claims 1 to 11.

13. The catalyst according to claim 12, characterized in that The active sites of the rare earth metal oxide and the noble metal of the catalyst are confined in the pure silicon molecular sieve structure, and the average particle size of the rare earth oxide-noble metal clusters is less than 4 nm.

14. Use of the rare earth oxide-noble metal catalyst for hydrogen isotope oxidation according to claim 12 or 13 in hydrogen isotope catalytic oxidation.