Efficient flotation separation method for coal byproducts
Through high shear slurry adjustment technology and the use of composite collectors, the problem of separation of coal gasified slag and liquefied slag raffinate has been solved, efficient carbon ash separation and resource utilization have been achieved, the dosage of drugs has been reduced, and the flotation has been significantly improved. Efficiency and resource utilization.
Patent Information
- Application Number
- CN202411406326.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-24
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to efficiently separate carbon and ash in coal gasified slag and liquefied slag raffinate, resulting in waste of resources and environmental pollution.
The coal by-products are mixed with water by-products and water by high shear slurry adjustment technology, and the composite collector and foaming agent are added to achieve full mixing and separation of gasified slag and liquefied slag raffinate through high-speed slurry adjustment and scraping process. Reduce the dosage of the drug and improve the flotation efficiency.
The carbon ash separation between gasified slag and liquefied slag raffinate is effectively achieved, the amount of flotation agent is reduced, the resource utilization rate is improved, environmental pollution is reduced, and resource utilization is achieved.
Smart Images

Figure CN119034947A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste fractionation and utilization, and in particular to a high-efficiency flotation separation method for coal by-products. Background Art
[0002] At present, efficient and clean utilization has become the focus of coal development. Against this background, coal gasification technology has developed rapidly and occupies a very important position in the energy industry. Gasification slag is a large waste generated in the coal gasification process, with an annual emission of tens of millions of tons. Direct coal liquefaction is the process of converting coal and hydrogen into liquid hydrocarbon fuel through hydrocracking under high temperature (about 400°C), high pressure (18-19MPa) and catalyst. With coal liquefaction slag as raw material, liquid mixture (extract) and solid slag (residue) are obtained by solvent extraction. Such materials are mostly landfilled or piled up, occupying a large amount of land, wasting land resources and releasing harmful waste gas to pollute the environment. The heavy metal leachate contained in the gasification slag and liquefied slag residue will also cause soil, surface water and groundwater pollution, seriously affecting the ecological environment.
[0003] In order to solve the resource utilization of gasification slag, according to the different physical and chemical properties of the mineral composition of gasification slag, flotation separation methods and equipment can be used to enrich and separate the target minerals. The obtained product has good adsorption properties. Wu Siping et al. conducted a flotation test on Yulin gasification slag. Under the conditions of 30kg / t diesel and 10kg / t of octanol, a refined carbon with a yield of 11.06% and an ash content of 28.23% can be obtained. Hu Junyang et al. and Liu Dongxue et al. used kerosene and No. 2 oil as flotation agents, respectively, and floated out refined carbon with a loss on ignition of 88.92% and a carbon content of 85.03%, with yields of 16.12% and 21.81%, respectively.
[0004] The surface of coal gasification slag contains a large number of oxygen-containing functional groups, strong hydrophilicity, poor floatability and large specific surface area, with many micropores and a well-developed pore structure, resulting in a large amount of reagent adsorption during flotation. The surface of the coal liquefaction slag residue is covered with a layer of oily extractant. The presence of the organic extractant makes the residue particles have a certain degree of adhesion and strong hydrophobicity, so that the carbon and ash in the liquefied slag residue cannot be effectively separated.
[0005] Therefore, how to efficiently flotation separate coal by-products has become an urgent problem that needs to be solved by technicians in this field. Summary of the invention
[0006] The purpose of the present invention is to provide a flotation separation method for coal by-products, which realizes the resource utilization, differentiated quality and high-quality utilization of gasification slag and liquefied slag extract residue by linkage and complementation between the two solid wastes, gasification slag and liquefied slag extract residue, adopts a combined sorting technology, and utilizes the characteristics of the physical and chemical properties of the two to separate the carbon from the ash, so as to solve the problems existing in the above-mentioned prior art.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] One of the technical solutions of the present invention is to provide a method for the efficient flotation separation of coal by-products, the steps comprising:
[0009] The coal by-products and water are mixed, and high shear slurry is used to obtain slurry, and then air is introduced to obtain concentrate and tailings through scraping and foaming; wherein a composite collector and a frother are sequentially added during the high shear slurrying process;
[0010] The coal by-product is a mixture of gasified slag and liquefied slag residue.
[0011] Furthermore, the mass ratio of the gasified slag to the liquefied slag residue in the coal by-product is 1-3:1-3.
[0012] Furthermore, the rotation speed of the high shear slurry adjustment is 6000-9000 rpm, and the time is 5-10 min.
[0013] Furthermore, the concentration of the slurry is 30 g / L.
[0014] Furthermore, the composite collector is a mixture of natural lipids and non-polar hydrocarbon oil in a mass ratio of 2:3, or a mixture of non-ionic surfactant and non-polar hydrocarbon oil in a mass ratio of 1:1.
[0015] Preferably, the natural lipid mixture and the non-polar hydrocarbon oil are cyclohexane acid and kerosene; and the non-ionic surfactant and the non-polar hydrocarbon oil are OP-10 and kerosene.
[0016] Furthermore, the dosage of the composite collector is 10-11 kg / t.
[0017] Furthermore, the foaming agent is octanol, and the dosage is 5 kg / t.
[0018] Furthermore, the air introduction rate is 0.3 m / s. 3 / h.
[0019] The second technical solution of the present invention is to provide a method for reducing the amount of flotation reagent used in flotation separation of gasified slag, the steps comprising:
[0020] The gasified slag and the liquefied slag residue are mixed evenly, and then mixed with water for high shear slurry adjustment to obtain ore slurry, and then air is introduced to obtain concentrate and tailings through scraping and bubbling; wherein, a composite collector and a frother are added in sequence during the high shear slurry adjustment process.
[0021] Furthermore, the mass ratio of the gasified slag to the liquefied slag residue is 1-3:1-3.
[0022] Furthermore, the rotation speed of the high shear slurry adjustment is 6000-9000 rpm, and the time is 5-10 min.
[0023] Furthermore, the concentration of the slurry is 30 g / L.
[0024] Furthermore, the composite collector is a mixture of natural lipids and non-polar hydrocarbon oil in a mass ratio of 2:3, or a mixture of non-ionic surfactant and non-polar hydrocarbon oil in a mass ratio of 1:1.
[0025] Preferably, the natural lipid mixture and the non-polar hydrocarbon oil are cyclohexane acid and kerosene; and the non-ionic surfactant and the non-polar hydrocarbon oil are OP-10 and kerosene.
[0026] Furthermore, the dosage of the composite collector is 10-11 kg / t.
[0027] Furthermore, the foaming agent is octanol, and the dosage is 5 kg / t.
[0028] Furthermore, the air introduction rate is 0.3 m / s. 3 / h.
[0029] The third technical solution of the present invention is to provide a method for improving the flotation separation effect of liquefied slag residue, the steps comprising:
[0030] The gasified slag and the liquefied slag residue are mixed evenly, and then mixed with water for high shear slurry adjustment to obtain ore slurry, and then air is introduced to obtain concentrate and tailings through scraping and bubbling; wherein, a composite collector and a frother are added in sequence during the high shear slurry adjustment process.
[0031] Furthermore, the mass ratio of the gasified slag to the liquefied slag residue is 1-3:1-3.
[0032] Furthermore, the rotation speed of the high shear slurry adjustment is 6000-9000 rpm, and the time is 5-10 min.
[0033] Furthermore, the concentration of the slurry is 30 g / L.
[0034] Furthermore, the composite collector is a mixture of natural lipids and non-polar hydrocarbon oil in a mass ratio of 2:3, or a mixture of non-ionic surfactant and non-polar hydrocarbon oil in a mass ratio of 1:1.
[0035] Preferably, the natural lipid mixture and the non-polar hydrocarbon oil are cyclohexane acid and kerosene; and the non-ionic surfactant and the non-polar hydrocarbon oil are OP-10 and kerosene.
[0036] Furthermore, the dosage of the composite collector is 10-11 kg / t.
[0037] Furthermore, the foaming agent is octanol, and the dosage is 5 kg / t.
[0038] Furthermore, the air introduction rate is 0.3 m / s. 3 / h.
[0039] The present invention discloses the following technical effects:
[0040] The present invention utilizes high shear slurry adjustment followed by flotation to achieve carbon-ash separation of gasified slag and liquefied slag residue. By adjusting high shear slurry adjustment and flotation operating parameters and process flow, a predetermined separation effect is achieved, and carbon-ash separation of liquefied slag residue can be effectively achieved, as well as reducing the amount of reagent used in conventional flotation of gasified slag.
[0041] The present invention adds a collector during the high-shear slurry adjustment process, and fully mixes the gasified slag and the liquefied slag extract residue through high-speed slurry adjustment, thereby avoiding the obstruction of the mineral surface film in the water environment, allowing the collector molecules or droplets to preferentially adhere and spread on the surface, increasing the contact area of interaction between particles, and promoting the adsorption of the collector on the surface, thereby reducing the dosage of the reagent, improving the flotation efficiency, and saving costs.
[0042] The collector selected by the present invention is a composite collector, one of which is a natural lipid mixture and a non-polar hydrocarbon oil (cyclohexane acid and kerosene) compounded at an optimal mass ratio of 2:3 for flotation efficiency, introducing polar groups, reducing the amount of reagents used, and thus improving the flotation effect; the other is a non-ionic surfactant and a non-polar hydrocarbon oil (OP-10 and kerosene) compounded at an optimal mass ratio of 1:1 for flotation efficiency, decomposing the oil into very fine particles and driving the dirt formed by the dirt off the surface of the liquefied slag residue and emulsifying it in water, which can be removed by dilution, reducing the surface tension of water and generating foam, which can not only promote the separation of liquefied slag residue and carbon ash and "blocking holes" of gasified slag, but also replace the foaming agent, thereby reducing the flotation process, reducing consumption and realizing the quality-separation utilization of gasified slag and liquefied slag residue, turning waste into treasure.
[0043] High shear slurry mixing technology is used to fully mix the gasified slag and liquefied slag residue, increase the contact area of the interaction between particles, reduce the effects of dipoles and hydrogen bonds between particles, and reduce internal friction. It can not only make the particles collide with each other and disperse, but also increase the chance of particles merging with each other. Since the liquefied slag residue has fine particles and disperses under high shear, part of the liquefied slag residue can enter the pores of the gasified slag and "block the pores" of the gasified slag, thereby reducing the amount of reagents used for separating the carbon ash from the gasified slag and improving the utilization rate of flotation reagents. The natural hydrophilicity of the gasified slag drives the hydrophobic liquefied slag residue into the water phase, which can promote the contact between the liquefied slag residue particles and the reagent, thereby promoting the separation of its carbon ash. It can significantly solve the problem that the liquefied slag residue is completely floating in the water phase and is not easy to interact with the reagent, and provide an effective way for the resource utilization of the two. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 It is a process flow chart of the present invention;
[0046] Figure 2 This is a microscopic picture of the liquefied slag residue entering the pores of the gasified slag in Example 1. DETAILED DESCRIPTION
[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0048] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0051] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0052] Figure 1 It is a process flow chart of the present invention.
[0053] The raw materials and reagents used in the specific implementation scheme of the present invention are all commercially available products, and the acquisition methods do not affect the realization of the technical effects.
[0054] The particle size of the gasified slag used in the specific embodiment of the present invention is D(10)6.22μm, D(50)49.2μm, D(90)157μm, and the BET specific surface area is 36.2637m 2 / g, the average pore size is 5.88nm, and the particle sizes of the liquefied slag residue used are D(10)4.17μm, D(50)12.1μm, and D(90)34.7μm.
[0055] Example 1
[0056] The steps of the efficient flotation separation method of coal by-products are:
[0057] The gasified slag and the liquefied slag residue were mixed evenly in a mass ratio of 1:1, and an appropriate amount of water (the pulp concentration was 30 g / L) was added. The high-speed disperser (9000 rpm) was turned on to start high-shear slurry mixing. After 3 minutes of high-shear slurry mixing, a composite collector (cyclohexane acid and kerosene in a mass ratio of 2:3, with a dosage of 11 kg / t) was added. The slurry mixing was continued for 3 minutes, and a foaming agent (octanol, with a dosage of 5 kg / t) was added. Then, aeration and scraping were started, and the aeration rate was 0.3 m / s. 3 / h, the scraping time is 3min, and concentrate and tailings are obtained.
[0058] Figure 2This is a microscopic image of the liquefied slag residue entering the pores of the gasified slag in Example 1. Figure 2 It can be seen that part of the liquefied slag extract can enter the pores of the gasified slag and "block the pores" of the gasified slag, thereby reducing the amount of reagents used for separating carbon from ash in the gasified slag and improving the utilization rate of flotation reagents.
[0059] Example 2
[0060] The steps of the efficient flotation separation method of coal by-products are as follows (reducing the dosage of reagents):
[0061] The gasified slag and the liquefied slag extract were mixed evenly in a mass ratio of 1:1, and an appropriate amount of water (the pulp concentration was 30 g / L) was added. The high-speed disperser (9000 rpm) was turned on to start high-shear slurry mixing. After 3 minutes of high-shear slurry mixing, a composite collector (cyclohexane acid and kerosene in a mass ratio of 2:3, with a dosage of 8 kg / t) was added. The slurry mixing was continued for 3 minutes and a foaming agent (octanol, with a dosage of 3 kg / t) was added. Then, aeration and scraping were started, and the aeration rate was 0.3 m / s. 3 / h, the scraping time is 3min, and concentrate and tailings are obtained.
[0062] Comparative Example 1
[0063] The steps of the flotation separation method of coal by-products are (single coal by-product):
[0064] Compared with Example 1, the only difference is that the gasified slag and liquefied slag raffinate are replaced with gasified slag of equal mass.
[0065] Comparative Example 2
[0066] The steps of the flotation separation method of coal by-products are (single coal by-product):
[0067] Compared with Example 1, the only difference is that the gasified slag and the liquefied slag extract are replaced by the liquefied slag extract of the same mass.
[0068] The concentrates and tailings obtained in Examples 1-2 and Comparative Examples 1-2 were filtered, dried, weighed, and ash content tested in sequence. The results are shown in Table 1.
[0069] Table 1
[0070]
[0071] From the comparison of the data in Table 1, it can be seen that in the present invention, the flotation of the gasified slag and the liquefied slag residue in a mass ratio of 1:1 is carried out after high shear slurry adjustment, compared with the flotation of the gasified slag alone, the concentrate yield is improved and the ash content of the concentrate is increased, indicating that part of the unseparated liquefied slag residue has entered the pores of the gasified slag, reducing the amount of flotation reagent. Compared with the flotation of the liquefied slag residue alone, the tailings yield and ash content of the present invention are greatly improved, and the carbon ash selective separation effect of the liquefied slag residue is remarkable.
[0072] Example 3
[0073] The steps of the efficient flotation separation method of coal by-products are:
[0074] The gasified slag and the liquefied slag residue were mixed evenly in a mass ratio of 2:1, and an appropriate amount of water (the pulp concentration was 30 g / L) was added. The high-speed disperser (9000 rpm) was turned on to start high-shear slurry mixing. After 3 minutes of high-shear slurry mixing, a composite collector (OP-10 and kerosene in a mass ratio of 1:1, with a dosage of 11 kg / t) was added. The slurry mixing was continued for 3 minutes and a foaming agent (octanol, with a dosage of 5 kg / t) was added. Then, aeration and scraping were started, and the aeration rate was 0.3 m / s. 3 / h, the scraping time is 3min, and concentrate and tailings are obtained.
[0075] Example 4
[0076] The steps of the efficient flotation separation method of coal by-products are as follows (reducing the dosage of reagents):
[0077] The gasified slag and the liquefied slag extract were mixed evenly in a mass ratio of 2:1, and an appropriate amount of water (the pulp concentration was 30 g / L) was added. The high-speed disperser (9000 rpm) was turned on to start high-shear slurry mixing. After 3 minutes of high-shear slurry mixing, a composite collector (OP-10 and kerosene in a mass ratio of 1:1, with a dosage of 8 kg / t) was added. The slurry mixing was continued for 3 minutes, and a foaming agent (octanol, with a dosage of 3 kg / t) was added. Then, aeration and scraping were started, and the aeration rate was 0.3 m / s. 3 / h, the scraping time is 3min, and concentrate and tailings are obtained.
[0078] Comparative Example 3
[0079] The steps of the flotation separation method of coal by-products are (single coal by-product):
[0080] Compared with Example 1, the only difference is that the gasified slag and liquefied slag raffinate are replaced with gasified slag of equal mass.
[0081] Comparative Example 4
[0082] The steps of the flotation separation method of coal by-products are (single coal by-product):
[0083] Compared with Example 1, the only difference is that the gasified slag and the liquefied slag extract are replaced by the liquefied slag extract of the same mass.
[0084] The concentrates and tailings obtained in Examples 3-4 and Comparative Examples 3-4 were filtered, dried, weighed, and ash content tested in sequence. The results are shown in Table 2.
[0085] Table 2
[0086]
[0087] It can be seen from the data in Table 2 that the flotation of the gasified slag and the liquefied slag residue at a mass ratio of 2:1 after high shear slurry adjustment in the present invention is compared with the flotation of the gasified slag alone, the concentrate yield is improved, and the concentrate ash content is increased, indicating that part of the unseparated liquefied slag residue has entered the pores of the gasified slag, thereby reducing the amount of flotation reagent. Compared with the flotation of the liquefied slag residue alone, the tailings yield and ash content are greatly improved, and the carbon ash selective separation effect of the liquefied slag residue is significant, which is basically consistent with the conclusion obtained in Example 1. It shows that under the target flotation reagent and reference raw material, it has a positive effect on the separation of gasified slag and liquefied slag residue.
[0088] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for efficient flotation separation of coal by-products, characterized in that the steps include: The coal by-products and water are mixed, and high shear slurry is used to obtain slurry, and then air is introduced to obtain concentrate and tailings through scraping and foaming; wherein a composite collector and a frother are sequentially added during the high shear slurrying process; The coal by-product is a mixture of gasified slag and liquefied slag residue.
2. The method according to claim 1, characterized in that The mass ratio of the gasified slag to the liquefied slag residue in the coal by-product is 1-3:1-3.
3. The method according to claim 1, characterized in that The high shear slurry adjustment has a rotation speed of 6000-9000 rpm and a time of 5-10 minutes.
4. The method according to claim 1, characterized in that The concentration of the slurry is 30 g / L.
5. The method according to claim 1, characterized in that The composite collector is a mixture of natural lipids and non-polar hydrocarbon oil in a mass ratio of 2:3, or a mixture of non-ionic surfactant and non-polar hydrocarbon oil in a mass ratio of 1:
1.
6. The method according to claim 5, characterized in that The natural lipid mixture and the non-polar hydrocarbon oil are cyclohexane acid and kerosene; the non-ionic surfactant and the non-polar hydrocarbon oil are OP-10 and kerosene.
7. The method according to claim 1, characterized in that The dosage of the composite collector is 10-11 kg / t; the foaming agent is 2-octanol, and the dosage is 5 kg / t.
8. The method according to claim 1, characterized in that The air flow rate is 0.3 m 3 / h.
9. A method for reducing the amount of flotation reagent used in flotation separation of gasified slag, characterized in that the steps include: The gasified slag and the liquefied slag residue are mixed evenly, and then mixed with water for high shear slurry adjustment to obtain ore slurry, and then air is introduced to obtain concentrate and tailings through scraping and bubbling; wherein, a composite collector and a frother are added in sequence during the high shear slurry adjustment process.
10. A method for improving the flotation separation effect of liquefied slag residue, characterized in that the steps include: The gasified slag and the liquefied slag residue are mixed evenly, and then mixed with water for high shear slurry adjustment to obtain ore slurry, and then air is introduced to obtain concentrate and tailings through scraping and bubbling; wherein, a composite collector and a frother are added in sequence during the high shear slurry adjustment process.