Preparation method of functionally graded material
By adjusting the plasma rotating electrode process to prepare metal particles of different sizes and mixing them with ceramic powder, and then hot-pressing and sintering them, functionally graded materials are formed. This solves the problem of balancing hardness and toughness in materials and achieves performance improvement in aerospace materials.
Patent Information
- Application Number
- CN202411275633.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-12
AI Technical Summary
Existing materials are difficult to balance high hardness and high toughness, and cannot meet the material performance requirements of the aerospace field.
By adjusting the rotational speed of the rotating electrode in the plasma rotating electrode process, metal particles of different sizes are prepared and mixed with ceramic powders of different proportions. These are then subjected to hot pressing and sintering to form functionally graded materials, thereby controlling the ceramic content gradient along the thickness direction of the material.
It achieves a gradient change in hardness and toughness along the thickness direction of the material, taking into account both high hardness and high toughness, and meeting the performance requirements of aerospace materials.
Smart Images

Figure CN119035556A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional gradient materials, and in particular to a method for preparing a functional gradient material. Background Art
[0002] In the field of aerospace, the requirements for material performance are high, requiring both high hardness and good toughness. However, the properties of materials in nature are often relatively stable, and it is impossible to take into account both hardness and toughness.
[0003] Therefore, a functionally gradient material that can balance hardness and toughness is needed. Summary of the invention
[0004] The embodiment of the present invention provides a method for preparing a functional gradient material, which can provide a functional gradient material having both hardness and toughness.
[0005] An embodiment of the present invention provides a method for preparing a functional gradient material, comprising: By adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, metal particles of different particle sizes can be prepared; The metal particles of different particle sizes are mixed with different amounts of ceramic powder to obtain multiple groups of mixed particles; wherein, in the multiple groups of mixed particles, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder; Performing a first hot pressing and sintering process on each group of the mixed particles to obtain a plurality of hot pressed layered bodies; A plurality of the hot-pressed layered bodies are stacked in the thickness direction in order of the ceramic content therein, and subjected to a second hot-pressing sintering treatment to obtain the functional gradient material.
[0006] In a possible design, before the second hot pressing and sintering process, the plurality of hot pressed layered bodies are subjected to ultrasonic treatment and high temperature hot air treatment.
[0007] In a possible design, the metal particles include titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.
[0008] In a possible design, the particle size of the ceramic powder is 5-10 μm.
[0009] In a possible design, the method of preparing metal particles of different particle sizes by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process includes: Determine the different size ranges of metal particles; According to the particle size range, the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm; According to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600~1200A; wherein the current and the rotation speed are inversely proportional; Micron-sized metal particles with different particle sizes of 5 to 20 μm are obtained.
[0010] In a possible design, each group of the mixed particles is subjected to a first hot pressing and sintering process to obtain a plurality of hot pressed layered bodies, including: A first hot pressing sintering treatment at different temperatures is performed on each group of the mixed particles; wherein the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.
[0011] In a possible design, in the multiple groups of mixed particles, the volume fraction of ceramic powder is 1 to 8.
[0012] In a possible design, the plurality of hot-pressed layered bodies are stacked in the thickness direction in the order of the ceramic content therein, and subjected to a second hot-pressing sintering process to obtain the functional gradient material, comprising: stacking a plurality of the hot-pressed laminates in order of ceramic content along a thickness direction; After a heat insulating layer is arranged on one side of the hot pressed layered body having the lowest ceramic content, a second hot pressing sintering process is performed to obtain the functional gradient material.
[0013] In a possible design, the temperature of the first hot pressing sintering includes 800-1200° C., and the pressure of the first hot pressing sintering includes 80-120 MPa.
[0014] In a possible design, the temperature of the second hot pressing sintering process is 950-1100° C., and the pressure is 100-150 MPa.
[0015] Compared with the prior art, the present invention has at least the following beneficial effects: In the present invention, metal particles with different particle sizes are first prepared by controlling the rotation speed of the plasma rotating electrode. The faster the rotation speed, the smaller the particle size of the metal particles, the faster the cooling rate, and the smaller the size of the crystal. Conversely, the slower the rotation speed, the larger the particle size of the metal particles, the slower the cooling rate, and the larger the size of the crystal. The smaller the size of the crystal, the higher the hardness, the larger the size of the crystal, and the better the toughness. In summary, by controlling the electrode rotation speed, small metal particles with small particle size and small crystal size and large metal particles with large particle size and large crystal size can be obtained. Metal particles of different particle sizes are mixed with ceramic powders of different volumes. The smaller the particle size of the metal particles, the higher the proportion of mixed ceramic powder, and multiple groups of mixed particles are obtained. In multiple groups of mixed particles, the smaller the particle size of the metal particles, the higher the proportion of ceramic powder in the mixed particles. The addition of ceramic powder can improve the ablation resistance of the material. At the same time, it can react at the boundary of the metal grains during sintering and forming. The generated ceramic body is filled and distributed at the boundary of the metal grains, increasing the hardness of the material itself. The higher the proportion of ceramic powder, the more obvious the hardness improvement. Conversely, the smaller the proportion of ceramic powder, the higher the toughness. Each group of mixed particles is subjected to a first hot pressing and sintering treatment to obtain a plurality of hot pressing layered bodies, and then the plurality of hot pressing layered bodies are stacked in the thickness direction in the order of the ceramic content therein, and subjected to a second hot pressing and sintering treatment to obtain a functional gradient material. The obtained material has different ceramic contents and different crystal sizes along the thickness direction, with one side having a small crystal size, a high ceramic content, and high hardness, and the other side having a large crystal size, a small ceramic content, or even no ceramic, and good toughness, and the hardness and toughness of the middle part change gradiently. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 It is a flow chart of a method for preparing a functional gradient material provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0019] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance; unless otherwise specified or explained, the term "multiple" refers to two or more; the terms "connected" and "fixed" should be understood in a broad sense, for example, "connected" can be a fixed connection, a detachable connection, an integral connection, or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0020] In the description of this specification, it should be understood that the directional words such as "upper" and "lower" described in the embodiments of the present invention are described at the angles shown in the drawings and should not be understood as limiting the embodiments of the present invention. In addition, in the context, it should also be understood that when it is mentioned that an element is connected to another element "upper" or "lower", it can not only be directly connected to another element "upper" or "lower", but also indirectly connected to another element "upper" or "lower" through an intermediate element.
[0021] Please refer to Figure 1 , an embodiment of the present invention provides a method for preparing a functional gradient material, comprising: By adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, metal particles of different particle sizes can be prepared; The metal particles of different particle sizes are mixed with different amounts of ceramic powder to obtain multiple groups of mixed particles; wherein, in the multiple groups of mixed particles, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder; Performing a first hot pressing and sintering process on each group of mixed particles to obtain a plurality of hot pressed layered bodies; A plurality of hot-pressed layered bodies are stacked in the thickness direction in order of the ceramic content therein, and subjected to a second hot-pressing sintering treatment to obtain a functional gradient material.
[0022] In the present invention, metal particles with different particle sizes are first prepared by controlling the rotation speed of the plasma rotating electrode. The faster the rotation speed, the smaller the particle size of the metal particles, the faster the cooling rate, and the smaller the size of the crystal. Conversely, the slower the rotation speed, the larger the particle size of the metal particles, the slower the cooling rate, and the larger the size of the crystal. The smaller the size of the crystal, the higher the hardness, the larger the size of the crystal, and the better the toughness. In summary, by controlling the electrode rotation speed, small metal particles with small particle size and small crystal size and large metal particles with large particle size and large crystal size can be obtained. Metal particles of different particle sizes are mixed with ceramic powders of different volumes. The smaller the particle size of the metal particles, the higher the proportion of mixed ceramic powder, and multiple groups of mixed particles are obtained. In multiple groups of mixed particles, the smaller the particle size of the metal particles, the higher the proportion of ceramic powder in the mixed particles. The addition of ceramic powder can improve the ablation resistance of the material. At the same time, it can react at the boundary of the metal grains during sintering and forming. The generated ceramic body is filled and distributed at the boundary of the metal grains, increasing the hardness of the material itself. The higher the proportion of ceramic powder, the more obvious the hardness improvement. Conversely, the smaller the proportion of ceramic powder, the higher the toughness. Each group of mixed particles is subjected to a first hot pressing and sintering treatment to obtain a plurality of hot pressing layered bodies, and then the plurality of hot pressing layered bodies are stacked in the thickness direction in the order of the ceramic content therein, and subjected to a second hot pressing and sintering treatment to obtain a functional gradient material. The obtained material has different ceramic contents and different crystal sizes along the thickness direction, with one side having a small crystal size, a high ceramic content, and high hardness, and the other side having a large crystal size, a small ceramic content, or even no ceramic, and good toughness, and the hardness and toughness of the middle part change gradiently.
[0023] It should be noted that the large-size metal particles may be mixed with a small amount of ceramic powder or may not be mixed with the ceramic powder. The above-mentioned different amounts of ceramic powder include 0-content ceramic powder.
[0024] In some embodiments of the present invention, before the second hot pressing and sintering process, the plurality of hot pressed layered bodies are subjected to ultrasonic treatment and high temperature hot air treatment.
[0025] In this embodiment, before the second hot pressing sintering treatment, in order to ensure the bonding strength and product quality, the multiple hot pressed layered bodies are ultrasonically treated to disperse the particles, stains or dust that may exist on their surfaces, and then high-temperature hot air is used to remove the dispersed particles, stains or dust.
[0026] In some embodiments of the present invention, the metal particles include titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.
[0027] In this embodiment, the titanium alloy has the characteristics of high temperature resistance, excellent mechanical properties and light weight, and is suitable for the aerospace field.
[0028] In this embodiment, the ceramic powder containing boron, carbon and / or nitrogen elements can react with titanium to obtain a ceramic body with increased hardness.
[0029] In some embodiments of the present invention, the particle size of the ceramic powder is 5-10 μm.
[0030] In this embodiment, the particle size of the ceramic powder is in the range of 5 to 10 μm, which can be well mixed and wrapped with the metal particles, increase the contact surface between the metal particles and the ceramic powder, and increase the efficiency of the combination or reaction.
[0031] In some embodiments of the present invention, metal particles of different particle sizes are prepared by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, including: Determine the different size ranges of metal particles; According to the particle size range, the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm; According to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600~1200A; wherein the current and the rotation speed are inversely proportional; Micron-sized metal particles with different particle sizes of 5 to 20 μm are obtained.
[0032] In this embodiment, the rotation speed can be controlled to be 8000~10000rpm, 18000~20000rpm, and 30000~35000rpm, respectively, and the three rotation speeds correspond to 1000~1200A, 800~1000A, and 600~800A, respectively. The higher the current, the higher the temperature of the electrode, the higher the melting degree of the metal material, the higher the melting degree, the larger the particles thrown out, and in addition, the slower the rotation speed, the larger the particles thrown out by the centrifugal force. Therefore, low rotation speed combined with high current can obtain metal particles with large particle size, and high rotation speed combined with low current can obtain metal particles with small particle size.
[0033] Of course, you can also set more different speeds between 8000~35000rpm according to your needs to obtain metal particles of more different particle sizes. The current can also be adaptively adjusted according to different speeds.
[0034] In some embodiments of the present invention, each group of mixed particles is subjected to a first hot pressing and sintering process to obtain a plurality of hot pressed layered bodies, including: Each group of mixed particles is subjected to a first hot pressing sintering treatment at different temperatures; wherein, the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.
[0035] In the present application, the temperature of the first hot pressing sintering treatment affects the degree of recrystallization of the metal. The higher the temperature, the better the degree of recrystallization and the larger the resulting grains. When the temperature is low, the degree of metal recrystallization is low or no recrystallization occurs. Therefore, by controlling the temperature of the first hot pressing sintering treatment at a higher temperature, the mixed particles of large metal grains can be sintered and the grains can be further enlarged; by controlling the first sintering temperature at a lower temperature, the mixed particles are only combined and compacted with each other, and no or little recrystallization occurs, so that after the mixed particles of small metal grains are sintered, the grains remain at a smaller degree.
[0036] In some embodiments of the present invention, in the plurality of groups of mixed particles, the volume fraction of the ceramic powder is 1-8.
[0037] In some embodiments of the present invention, multiple hot-pressed layered bodies are stacked in the thickness direction in order of ceramic content, and subjected to a second hot-pressing sintering process to obtain a functional gradient material, including: stacking a plurality of hot-pressed laminates in order of ceramic content along a thickness direction; After a heat insulating layer is provided on one side of the hot pressed layered body having the lowest ceramic content, a second hot pressing sintering treatment is performed to obtain a functional gradient material.
[0038] In this embodiment, after a heat-insulating layer is provided on one side of the hot-pressed layered body with the lowest ceramic content, the heating rate is slow during the second hot-pressing sintering, but with the passage of time, it can still reach a temperature (900°C) that can transform the titanium crystals from a close-packed hexagonal structure to a body-centered cubic structure. With the end of the second hot-pressing sintering, the temperature begins to gradually decrease. However, due to the presence of the heat-insulating layer, the cooling rate of the part with a low ceramic content is slow. The cooling rate is related to the content of body-centered cubic structure crystals. The slower the cooling rate, the lower the content of body-centered cubic structure crystals, and the stronger the toughness of the material. The faster the cooling rate, the higher the content of body-centered cubic structure crystals, and the stronger the hardness of the material.
[0039] It should be noted that although the second hot pressing sintering treatment also causes recrystallization, the size relationship between the larger crystals and the smaller crystals remains unchanged after both are recrystallized. In addition, ceramic phases are distributed at the boundaries of the small crystals inside the hot pressing layered body of the smaller crystals, which limits the degree of recrystallization. Therefore, only part of the crystals inside the hot pressing layered body of the smaller crystals are recrystallized, which has little effect on the change of the overall crystal particles.
[0040] In some embodiments of the present invention, the temperature of the first hot pressing sintering includes 800-1200° C., and the pressure of the first hot pressing sintering includes 80-120 MPa.
[0041] In some embodiments of the present invention, the temperature of the second hot pressing sintering process is 950-1100° C., and the pressure is 100-150 MPa.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a functional gradient material, characterized in that: include: By adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, metal particles of different particle sizes can be prepared; The metal particles of different particle sizes are mixed with different amounts of ceramic powder to obtain multiple groups of mixed particles; wherein, in the multiple groups of mixed particles, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder; Performing a first hot pressing and sintering process on each group of the mixed particles to obtain a plurality of hot pressed layered bodies; A plurality of the hot-pressed layered bodies are stacked in the thickness direction in order of the ceramic content therein, and subjected to a second hot-pressing sintering treatment to obtain the functional gradient material.
2. The preparation method according to claim 1, characterized in that: Before the second hot pressing and sintering process, the plurality of hot pressed layered bodies are subjected to ultrasonic treatment and high temperature hot air treatment.
3. The preparation method according to claim 1, characterized in that: The metal particles include titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.
4. The preparation method according to claim 1, characterized in that: The particle size of the ceramic powder is 5-10 μm.
5. The preparation method according to claim 1, characterized in that: The method of preparing metal particles of different particle sizes by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process comprises: Determine the different size ranges of metal particles; According to the particle size range, the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm; According to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600~1200A; wherein the current and the rotation speed are inversely proportional; Micron-sized metal particles with different particle sizes of 5 to 20 μm are obtained.
6. The preparation method according to claim 1, characterized in that: The first hot pressing and sintering treatment is performed on each group of the mixed particles to obtain a plurality of hot pressed layered bodies, including: A first hot pressing sintering treatment at different temperatures is performed on each group of the mixed particles; wherein the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.
7. The preparation method according to claim 1, characterized in that: In the plurality of groups of mixed particles, the volume fraction of the ceramic powder is 1 to 8.
8. The preparation method according to claim 1, characterized in that: The method of stacking a plurality of the hot-pressed layered bodies in the order of ceramic content along the thickness direction and performing a second hot-pressing sintering process to obtain the functional gradient material comprises: stacking a plurality of the hot-pressed laminates in order of ceramic content along a thickness direction; After a heat insulating layer is arranged on one side of the hot pressed layered body having the lowest ceramic content, a second hot pressing sintering process is performed to obtain the functional gradient material.
9. The preparation method according to claim 1, characterized in that: The temperature of the first hot pressing sintering is 800-1200° C., and the pressure of the first hot pressing sintering is 80-120 MPa.
10. The preparation method according to claim 1, characterized in that: The temperature of the second hot pressing sintering process is 950-1100° C., and the pressure is 100-150 MPa.
Citation Information
Patent Citations
Method for molding hard alloy functionally gradient materials
CN104874797A
Functional gradient aluminum-based composite material with multilevel gradient structure and preparation method thereof
CN107805728A
Hard alloy with gradient cobalt content and preparation method thereof
CN109321805A
Ceramic reinforced double-gradient composite material based on laser melting deposition and preparation method thereof
CN116786841A
Die made of composite material
JP2000355705A