Production and preparation method of pure titanium or titanium alloy composite continuous pipe

By adopting oblique bevel milling, welding and nano-treating techniques in continuous pipe production, combining carbon fiber layer and epoxy resin layer, the preparation of light and corrosion-resistant self-perceptual composite pipes is achieved, and corrosion in ultra-deep wells is solved. The self-weight problem meets the need for lightweight and real-time supervision.

CN119035998APending Publication Date: 2024-11-29SHAANXI RAILWAY INST
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411459682.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing continuous pipes have corrosion damage and self-weight problems in ultra-deep wells, and lack light and real-time supervision production technology, which cannot meet the production requirements of carbon fiber/pure titanium or titanium alloy composite pipes.

Method used

The strip is made of pure titanium or titanium alloy raw materials, and it is made of oblique bevel milling, head welding, nano-treating, continuous roll progressive pressing, welding seamless treatment, spraying epoxy resin layer and winding carbon fiber layer, combined with online Sensor monitoring to form self-perception and self-feedback composite pipes.

Benefits of technology

Prepare lightweight and corrosion-resistant composite continuous pipes, which can monitor downhole conditions in real time and avoid safety accidents. They are suitable for marine oil and gas reservoirs and ultra-deep well oil and gas fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035998A_ABST
    Figure CN119035998A_ABST
Patent Text Reader

Abstract

According to the production and preparation method of the pure titanium or titanium alloy composite continuous pipe, pure titanium or titanium alloy raw materials are longitudinally sheared to form strips with the same width size, the strips are subjected to head and tail butt welding after being subjected to oblique groove milling, shot blasting treatment is conducted on the outer surfaces of the welded strips, and the pure titanium or titanium alloy composite continuous pipe is obtained. Then the strip is pressed into a tubular shape through a continuous row roller progressive pressing forming method, welding is carried out on joint points of tubular forming, seamless treatment is carried out on welding seams, then a sensor is arranged on the outer surface of the pipe, carbon fiber filaments and strips are wound on the outer surface of the pipe to form a carbon fiber layer, and online continuous dipping and curing treatment is carried out on the whole pipe with the carbon fiber layer. And finally, winding on a winding drum device with a certain diameter size to finish the preparation. According to the invention, the composite continuous pipe with relatively light total weight, excellent corrosion resistance and self-sensing and self-feedback functions can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of continuous pipes, and in particular relates to a production method for pure titanium or titanium alloy composite continuous pipes. Background Art

[0002] Coiled tubing (CT) is a type of pipe that is continuously produced through special preparation technology and can be up to 10,000 meters long. Coiled tubing is widely used in industrial production and people's daily life, for example, in submarine optical cables, cables in cross-sea bridges and tunnels, oil and gas well maintenance, drilling, logging, oil and gas transportation and other operations. With the development and utilization of deep-well oil and gas reservoir resources and offshore oil and gas reservoir resources, and the complex working environment, higher requirements are placed on oil and gas extraction equipment. Currently, the existing coiled tubing is mainly made of carbon steel, followed by high-alloy coiled tubing, and pure titanium or titanium alloy coiled tubing is basically blank. However, carbon steel continuous pipes are mainly subject to corrosion damage. When used in ultra-deep wells, they are prone to shrinkage and cracks at the wellhead due to their heavy weight underground. High-alloy continuous pipes, although they solve the problem of corrosion resistance, are still a serious problem in ultra-deep wells due to their heavy weight. Although pure titanium or titanium alloy continuous pipes can perfectly solve the problems of corrosion and heavy weight, they cannot monitor and detect the working conditions underground and the changes in pipe wall thickness during use, and some minor problems in the early stage cannot be discovered in time. Therefore, lightweight, reliable, and real-time monitorable continuous pipe products are the mainstream demand direction of the future continuous pipe market.

[0003] However, there is no report or news on the research and development, production, and preparation of continuous pipe products that are both lightweight and can be monitored in real time in the pipe market, nor has there been any related technology or product launched, and its systematic production and preparation technology is still in a blank period. The existing production and preparation methods of conventional continuous pipes and high-alloy continuous pipes (continuous roller progressive pressing + high-frequency resistance welding + induction heat treatment) cannot adapt to and meet the production and preparation requirements of carbon fiber / pure titanium or titanium alloy composite continuous pipes in terms of welding methods, process measures, and heat treatment. Therefore, the present invention proposes a production and preparation method for pure titanium or titanium alloy composite continuous pipes. Summary of the invention

[0004] The purpose of the present invention is to provide a production method for pure titanium or titanium alloy composite continuous pipes, which can produce composite continuous pipes with relatively lighter total weight, excellent corrosion resistance, self-sensing and self-feedback functions.

[0005] The technical scheme adopted by the present invention is a production and preparation method of pure titanium or titanium alloy composite continuous pipes, which comprises longitudinally shearing pure titanium or titanium alloy raw materials to form strips of the same width, performing oblique groove milling on the strips and then butt welding the heads and tails, shot peening the outer surface of the strips after welding, pressing the strips into a tube by a continuous roller progressive pressing method, welding the joints of the tube and making the welds seamless, then arranging sensors on the outer surface of the pipes and winding carbon fiber filaments and strips to form a carbon fiber layer, performing online continuous impregnation and curing treatments on the overall pipe forming the carbon fiber layer, and finally winding the pipes on a reel device of a certain diameter to complete the preparation.

[0006] The present invention is also characterized in that The specific steps include: Step 1, slitting the pure titanium or titanium alloy raw material roll into strips with the same width; Step 2, performing oblique “I”-shaped groove milling on the head and tail of two strips of the same width; Step 3, butt welding the pure titanium or titanium alloy strip that has completed the head and tail bevel processing and performing seamless heat treatment on the weld; Step 4, performing "I"-shaped groove milling on both longitudinal sides of the pure titanium or titanium alloy strip that has been butt-welded, and performing nano-treatment on the outer surface of the strip using laser shock peening technology; Step 5, using a continuous roller progressive pressing method to continuously press the pure titanium or titanium alloy strip that has completed the nano-treatment into a continuous tube online; Step 6, performing online continuous longitudinal seam welding at the joint point of the tubular forming; Step 7, continuously scraping the inner and outer weld excess heights after welding, and performing seamless processing using a linear special heat treatment device; Step 8, spraying an epoxy resin layer online on the outer surface of the pipe body, applying adhesive and inserting a temperature monitoring sensor, a wall thickness monitoring sensor and a pressure monitoring sensor; Step 9, performing online continuous tubular winding and weaving of carbon fiber filaments and ribbons on the outer surface of the tube body to complete the preparation of the carbon fiber layer; Step 10, the entire tube body is sequentially impregnated and cured to prepare a carbon fiber-coated pure titanium or titanium alloy composite continuous tube; Step 11, continuously winding the prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube on a reel device with a certain diameter size to complete the preparation.

[0007] In step 1, the pure titanium or titanium alloy raw material coil is any one of TA1, TA2, TA3, TA4, TA5, TA6, TA7, TA8, TA8-1, TA9, TA9-1, TA10, TA11, TA15, TA17, TA18, TC1, TC2, TC3, TC4 and TC4ELI, the thickness of the pure titanium or titanium alloy raw material coil is 1.5 mm to 5.0 mm, and the width of the strip after longitudinal shearing is 80 mm to 600 mm; Step 2 is specifically as follows: the head of the previous coil of strip and the tail of the next coil of strip are subjected to an "I"-shaped groove milling process with an angle of 30 to 100 degrees to expose a fresh metallic luster.

[0008] Step 3 specifically comprises: using a plasma arc welding method or a laser welding method to perform oblique butt welding of the strip to form an oblique butt weld, and simultaneously performing inert gas protection within a range of length×width=200mm×20mm near the high temperature area of ​​the front and back sides of the strip; In step 3, the seamless heat treatment of the weld specifically includes scraping the oblique butt weld with a high temperature resistant and sticking resistant hard alloy scraper and vacuum seamless heat treatment of the oblique weld with a linear special heat treatment device to ensure that the weld is flat and consistent with the parent material; The vacuum seamless heat treatment process of the weld is: firstly, rapidly heat to 950℃~1000℃ for heat treatment, keep warm for 30s~120s, then water cool to room temperature, then rapidly heat to 550℃~650℃, keep warm for 30s~120s, then naturally cool to room temperature; Step 4 is specifically as follows: using a special tool to continuously perform online "I"-shaped groove milling on both longitudinal sides of the pure titanium or titanium alloy strip, without edge wrinkles and defects; and using laser impact shot peening technology to perform nano-treatment on the outer surface of the pure titanium or titanium alloy strip, with a coverage rate of 100%.

[0009] Step 5 is specifically as follows: firstly, the two longitudinal edges of the strip are continuously bent and formed by the first set of special rollers, then the strip is continuously bent and deformed from the edge to the inside by the subsequent special rollers, and finally, an external special roller pair is used to extrude and form the strip from the outside into a tube.

[0010] Step 6 is specifically as follows: a plasma arc welding method or a laser welding method is used to perform continuous longitudinal seam welding at the joint point to form a longitudinal weld of the pure titanium or titanium alloy pipe, the groove gap at the joint point is 0, the lateral extrusion amount is 0.3mm~1.0mm, and inert gas protection is simultaneously performed within a range of length×width=200mm×20mm near the high temperature zone of the inner and outer welds of the pipe.

[0011] Step 7 is as follows: a high temperature resistant and sticky resistant carbide scraper is used to continuously scrape the longitudinal seam excess height. The seamless heat treatment process is as follows: firstly rapidly heat to 950°C~1000°C for heat treatment, keep warm for 30s~120s and then cool to room temperature with water, then rapidly heat to 550°C~650°C, keep warm for 30s~120s and then naturally cool to room temperature.

[0012] In step 8, the temperature monitoring sensor, the wall thickness monitoring sensor and the pressure monitoring sensor are evenly arranged in sequence at equal angles along the circumference of the pipe body; The thickness of the carbon fiber layer in step 9 is 1 mm to 4 mm.

[0013] In step 10, a liquid resin solution is used for impregnation treatment, the impregnation temperature is 50° C. to 250° C., the impregnation time is 30s to 300s, and the curing treatment adopts a linear continuous curing treatment device.

[0014] The prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube is continuously wound on a reel device with a diameter of 800mm~2000mm. The end of the tube is locked with the reel outer frame device with a special lock, and the port is protected with a sealing ring.

[0015] The beneficial effects of the present invention are: The present invention provides a production and preparation method for pure titanium or titanium alloy composite continuous pipes. The technical method is reliable. The welding groove design, welding method determination, nano-processing, seamless processing, spraying epoxy resin layer, inserting sensors, carbon fiber layer preparation and other processes and the proposal of the whole production and preparation method are all based on the high-quality production of pure titanium or titanium alloy composite continuous pipes coated with carbon fiber; by spraying epoxy resin layer, inserting sensors, and carbon fiber layer preparation, the overall quality of the prepared composite pipe is lighter and the working environment of the pipe can be monitored in real time. Once the pipe equipment has abnormal conditions such as corrosion damage, it can be known in the first time, avoiding the occurrence of safety accidents while ensuring the operation efficiency; The composite continuous pipe prepared by the present invention is suitable for offshore oil and gas reservoir exploitation, long-distance submarine cable penetration, cross-sea bridge and tunnel pipelines and line facilities, and - It can be used for inland highly acidic deep wells and ultra-deep oil and gas fields with corrosive media such as etc., solve the corrosion and destructive problems of special pipe equipment such as marine environment oil and gas fields, cross-sea bridges and tunnels, and long-distance submarine cables, and fill the gap in the production and manufacturing technology of self-sensing pure titanium or titanium alloy composite continuous pipes, and is at the leading level in China. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic flow chart of the production method of the pure titanium or titanium alloy composite continuous pipe of the present invention; Figure 2This is a schematic diagram of the oblique butt welding of strips of the present invention; Figure 3 It is a schematic diagram of the tubular forming process of the present invention by progressive pressing of continuous rollers; Figure 4 It is a schematic cross-sectional view of the pure titanium or titanium alloy composite continuous pipe of the present invention.

[0017] In the figure, 1. the head of the previous roll of strip, 2. the tail of the next roll of strip, 3. the oblique butt weld, 4. the pure titanium or titanium alloy layer, 5. the epoxy coating, 6. the temperature monitoring sensor, 7. the wall thickness monitoring sensor, 8. the pressure monitoring sensor, 9. the carbon fiber layer. DETAILED DESCRIPTION

[0018] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0019] The production and preparation method of the pure titanium or titanium alloy composite continuous pipe of the present invention comprises the following steps: longitudinally shearing the pure titanium or titanium alloy raw material into strips of the same width, performing oblique groove milling on the strips and then performing head and tail butt welding, shot peening the outer surface of the strips after welding, pressing the strips into a tube by a continuous row of rollers progressive pressing method, welding the joints of the tube, arranging a sensor on the outer surface of the tube, and winding carbon fiber filaments and strips to form a carbon fiber layer 9, performing online continuous impregnation and curing treatment on the overall tube forming the carbon fiber layer 9, and finally winding the tube on a reel device of a certain diameter to complete the preparation.

[0020] The composite continuous pipe prepared by the present invention is suitable for offshore oil and gas reservoir exploitation, long-distance submarine cable penetration, cross-sea bridge and tunnel pipelines and line facilities, and - It can be used for inland highly acidic deep wells and ultra-deep oil and gas fields with corrosive media such as etc., solve the corrosion and destructive problems of special pipe equipment such as marine environment oil and gas fields, cross-sea bridges and tunnels, and long-distance submarine cables, and fill the gap in the production and manufacturing technology of self-sensing pure titanium or titanium alloy composite continuous pipes, and is at the leading level in China.

[0021] Example 1 The production method of the pure titanium or titanium alloy composite continuous pipe of the present invention is as follows: Figure 1 As shown, the specific steps include: Step 1, longitudinally shearing a pure titanium or titanium alloy raw material coil into strips of the same width; the pure titanium or titanium alloy raw material coil is any one of TA1, TA2, TA3, TA4, TA5, TA6, TA7, TA8, TA8-1, TA9, TA9-1, TA10, TA11, TA15, TA17, TA18, TC1, TC2, TC3, TC4 and TC4ELI, the thickness of the pure titanium or titanium alloy raw material coil is 1.5 mm to 5.0 mm, and the width of the strip after longitudinal shearing is 80 mm to 600 mm.

[0022] Step 2: Perform an oblique “I”-shaped groove milling process on the head and tail of two strips of the same width to expose a fresh metallic luster; Figure 2 As shown, the head 1 of the previous coil of strip and the tail 2 of the next coil of strip are subjected to an "I"-shaped groove milling process with an angle of 30 to 100 degrees to reveal a fresh metallic luster.

[0023] Step 3, the pure titanium or titanium alloy strip that has completed the head and tail bevel processing is subjected to the plasma arc welding (PAW) method or the laser welding (LBW) method to perform the strip oblique butt connection welding to form an oblique butt weld 3, and a single pure titanium or titanium alloy strip with a length of 10,000 meters is connected. The front and back sides of the strip are welded near the high temperature area within a range of length × width = 200 mm × 20 mm. Inert gas protection is simultaneously performed; The weld is heat treated to achieve seamlessness, including scraping the oblique butt weld 3 with a high temperature resistant and sticking resistant hard alloy scraper and vacuum seamless heat treatment of the oblique weld with a linear special heat treatment device, to ensure that the weld is level and consistent with the parent material; The specific process of vacuum seamless treatment is: first quickly heat to 950℃~1000℃, keep warm for 30s~120s, then water cool to room temperature, then quickly heat to 550℃~650℃, keep warm for 30s~120s, then naturally cool to room temperature.

[0024] Step 4: Perform "I"-shaped groove milling on both sides of the pure titanium or titanium alloy strip that has completed the butt welding connection. The groove extension reveals a fresh metallic luster without wrinkles or damage, and the outer surface of the strip is nano-processed using laser impact shot peening technology.

[0025] Specifically, a special tool is used to continuously perform online "I"-shaped groove milling on both longitudinal edges of pure titanium or titanium alloy strips, without edge wrinkles and defects; and laser shock peening technology is used to perform nano-treatment on the outer surface of pure titanium or titanium alloy strips, with a coverage rate of 100%.

[0026] Step 5, using a continuous row of rollers progressive pressing method to continuously press the butt-welded pure titanium or titanium alloy strip into a continuous tube online; specifically, Figure 3 As shown, the first set of special rollers are used to continuously bend the two longitudinal edges of the strip, then the subsequent special rollers are used to continuously bend and deform the strip from the edge to the inside, and finally an external special roller pair is used to extrude and form it from the outside into a tube.

[0027] Step 6, performing online continuous longitudinal seam welding at the joint point of the tubular forming.

[0028] Step 7, continuously scrape the excess height of the internal and external welds after welding, and use a linear special heat treatment device to perform seamless treatment.

[0029] Step 8, spray an epoxy resin layer online on the outer surface of the pipe body, apply adhesive and place a temperature monitoring sensor 6, a wall thickness monitoring sensor 7 and a pressure monitoring sensor 8; Figure 4 As shown, the temperature monitoring sensor 6, the wall thickness monitoring sensor 7 and the pressure monitoring sensor 8 are evenly arranged in sequence at equal angles along the circumference of the pipe body.

[0030] Step 9, performing online continuous tubular winding and weaving of carbon fiber filaments and ribbons on the outer surface of the tube body to complete the preparation of the carbon fiber layer 9, the thickness of the carbon fiber layer 9 is 1 mm to 4 mm; Step 10, the entire tube body is sequentially and continuously impregnated and cured online to prepare a carbon fiber-coated pure titanium or titanium alloy composite continuous tube; Step 11, continuously winding the prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube on a reel device with a certain diameter size to complete the preparation.

[0031] Example 2 On the basis of Example 1, in the production and preparation method of the pure titanium or titanium alloy composite continuous pipe of the present invention, step 6 adopts a plasma arc welding method or a laser welding method to perform continuous longitudinal seam welding at the joint point to form a longitudinal weld of the pure titanium or titanium alloy pipe, the groove gap at the joint point is 0, the lateral extrusion amount is 0.3mm~1.0mm, and the high temperature zone of the inner and outer welds of the pipe is near the length×width=200mm×20mm range. Inert gas protection is simultaneously performed; Step 7: Use a high temperature resistant and sticky resistant carbide scraper for continuous scraping. The specific process of seamless processing is: first quickly heat to 950℃~1000℃, keep warm for 30s~120s, then water cool to room temperature, then quickly heat to 550℃~650℃, keep warm for 30s~120s, then naturally cool to room temperature. Ensure that the weld structure and performance are consistent with the parent material.

[0032] In step 10, a liquid resin solution is used for impregnation treatment, the impregnation temperature is 50°C to 250°C, and the impregnation time is 30s to 300s, to ensure that the carbon fiber layer 9, the epoxy coating 5, and the outer surface of the pure titanium or titanium alloy layer 4 are completely impregnated with the epoxy resin solution. The curing treatment adopts a linear continuous curing treatment device to ensure that the liquid resin between the carbon fiber layer 9, the epoxy coating 5, and the outer surface of the pure titanium or titanium alloy layer 4 is completely cured.

[0033] Finally, the prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube is continuously wound on a reel device with a diameter of 800mm~2000mm. The end of the tube is locked with the reel outer frame device with a special lock, and the port is protected with a sealing ring.

[0034] Example 3 The production method of the pure titanium or titanium alloy composite continuous pipe of the present invention is specifically implemented according to the following steps: Step 1, longitudinally cutting a TC4 titanium alloy raw material roll with a wall thickness of 2.0 mm into a 280 mm wide strip; Step 2: Mill the head and tail of the front and rear strips into an "I"-shaped groove with an angle of 45°. The groove surface and the outer extension show a fresh metallic luster, and the groove edge has no wrinkles or defects. Step 3, the plasma arc welding (PAW) method is used to perform the strip oblique 45° butt welding, the gap is 0 mm, the longitudinal extrusion amount is 0.8 mm, and the inert gas protection is performed simultaneously in the range of length × width = 200 mm × 20 mm near the high temperature zone of the front and back sides of the strip. The welding parameters are shown in Table 1, and a TC4 titanium alloy strip with a total length of 6000 meters is connected; Alternatively, the laser welding method is used to perform butt welding of the strip at an angle of 45°, the longitudinal extrusion amount is 0.5 mm, and inert gas protection is performed simultaneously in the range of length × width = 200 mm × 20 mm near the high temperature zone of the front and back sides of the strip. The welding parameters are shown in Table 1, and a TC4 titanium alloy strip with a total length of 6000 meters is connected; Table 1 Strip oblique butt welding process parameters

[0035] Step 4: Use a high temperature resistant and sticky resistant carbide scraper to scrape the excess height of the oblique butt weld to ensure that the weld is flush with the base material; Step 5: Use a special heat treatment device to vacuum heat treat the oblique butt weld at a temperature of 980°C, a holding time of 120 seconds, and water cooling to room temperature. Then, quickly heat to 630°C, hold for 120 seconds, and naturally cool to room temperature to ensure that the weld and the parent material have consistent structure and performance. Step 6: Use a special tool to continuously perform “I”-shaped groove milling on both longitudinal sides of the pure titanium or titanium alloy strip online without edge wrinkles and defects; Step 7: Use laser impact peening technology to perform nano-treatment on the outer surface of pure titanium or titanium alloy strip, with a laser power density of 16GW / cm 2 , the laser pulse width is 15ns, the spot size is 4mm×4mm, and the coverage is 100%; Step 8: Use a continuous roller progressive pressing method. The forming process is as follows: Figure 3 As shown, the first set of special roller pressing wheels are used to continuously bend and deform the two longitudinal sides of the strip, and then the subsequent special roller pressing wheels are used to continuously bend and deform from the edge to the inside, and finally the external special roller pressing wheels are used to extrude and form from the outside to form a Ø89mm continuous tube; Step 9: Plasma arc welding (PAW) is used to perform continuous longitudinal seam welding at the joint point of the tubular forming. The groove gap at the joint point is 0, the lateral extrusion amount is 0.8 mm, and inert gas protection is performed simultaneously in the range of length × width = 200 mm × 20 mm near the welding high temperature zone inside and outside the pipe body. The welding parameter settings are shown in Table 2; Or, laser welding is used to perform continuous longitudinal seam welding at the joint point of tubular forming, the groove gap at the joint point is 0, the transverse extrusion amount is 0.5 mm, and inert gas protection is performed simultaneously within the range of length × width = 200 mm × 20 mm near the inner and outer welding high temperature zones of the pipe body. The welding parameter settings are shown in Table 2; Table 2 Longitudinal seam welding process parameters

[0036] Step 10: Use a high temperature resistant and sticky resistant carbide scraper to continuously scrape the inner and outer weld excess height to ensure that the weld is flush with the base material; Step 11: Use a special heat treatment device to perform continuous vacuum seamless heat treatment on the weld at a heat treatment temperature of 980°C, keep warm for 60 seconds, then cool with water, then quickly heat to 630°C, keep warm for 60 seconds, then cool with air, to ensure that the weld is consistent with the parent material in structure and performance; Step 12: Spray epoxy resin online continuously on the outer surface of the pipe body. The epoxy coating 5 has a thickness of 1.0 mm. Apply adhesive and place the temperature monitoring sensor 6, pipe wall thickness monitoring sensor 7 and pressure monitoring sensor 8 at the same time. Figure 4 As shown; Step 13, winding and weaving of online continuous carbon fiber layers, with a thickness of 3 mm; Step 14, online and continuously performing an impregnation treatment of the pure titanium or titanium alloy composite continuous pipe with a liquid resin solution, the immersion temperature is 200° C., the immersion time is 40 seconds, and the outer surface of the carbon fiber layer 9, the epoxy coating 5, and the pure titanium or titanium alloy layer 4 are completely impregnated with the epoxy resin solution; Step 15, subjecting the completely impregnated pure titanium or titanium alloy composite continuous pipe to an online continuous curing process to ensure that the liquid resin between the carbon fiber layer 9, the epoxy coating 5, and the outer surface of the pure titanium or titanium alloy layer 4 is completely cured; Step 16, rewinding the completely solidified pure titanium or titanium alloy composite continuous pipe with a specification of Ø89 mm×(2.0+4.0) mm×6000 m on a reel device with a diameter of 2000 mm; Step 17: The end of the pipe is locked with a special lock buckle and a reel outer frame device, and the end is protected with a sealing ring to obtain a new product of a single pure titanium or titanium alloy composite continuous pipe with a length of up to 6,000 meters.

[0037] The performance test results of the obtained pure titanium or titanium alloy composite continuous pipe are shown in Table 3.

[0038] Table 3 Performance test results of TC4 composite continuous pipe

Claims

1. Production and preparation method of pure titanium or titanium alloy composite continuous pipe, It is characterized in that Pure titanium or titanium alloy raw materials are longitudinally cut to form strips of the same width, the strips are subjected to oblique groove milling and then butt-welded at the head and tail, the outer surface of the strip after welding is shot peened, and then the strip is pressed into a tube by a continuous roller progressive pressing method, the joint points of the tube are welded and the weld is seamlessly processed, and then a sensor is arranged on the outer surface of the tube and carbon fiber filaments and strips are wound to form a carbon fiber layer (9), the overall tube forming the carbon fiber layer (9) is subjected to online continuous impregnation and curing treatment, and finally wound on a reel device of a certain diameter to complete the preparation.

2. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 1, It is characterized in that The specific steps include: Step 1, slitting the pure titanium or titanium alloy raw material roll into strips with the same width; Step 2, performing oblique "I"-shaped groove milling on the head and tail of two strips of the same width; Step 3, butt welding the pure titanium or titanium alloy strip that has completed the head and tail bevel processing and performing seamless heat treatment on the weld; Step 4, performing "I"-shaped groove milling on both sides of the pure titanium or titanium alloy strip that has been butt-welded, and performing nano-treatment on the outer surface of the strip using laser shock peening technology; Step 5, using a continuous roller progressive pressing method to continuously press the pure titanium or titanium alloy strip that has completed the nano-treatment into a continuous tube online; Step 6, performing online continuous longitudinal seam welding at the joint point of the tubular forming; Step 7, continuously scraping the inner and outer weld excess heights after welding, and performing seamless processing using a linear special heat treatment device; Step 8, spraying an epoxy resin layer online on the outer surface of the pipe body, applying adhesive and inserting a temperature monitoring sensor (6), a wall thickness monitoring sensor (7) and a pressure monitoring sensor (8); Step 9, performing online continuous tubular winding and weaving of carbon fiber filaments and ribbons on the outer surface of the tube body to complete the preparation of the carbon fiber layer (9); Step 10, the entire tube body is sequentially impregnated and cured to prepare a carbon fiber-coated pure titanium or titanium alloy composite continuous tube; Step 11, continuously winding the prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube on a reel device with a certain diameter size to complete the preparation.

3. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that In the step 1, the pure titanium or titanium alloy raw material coil is any one of TA1, TA2, TA3, TA4, TA5, TA6, TA7, TA8, TA8-1, TA9, TA9-1, TA10, TA11, TA15, TA17, TA18, TC1, TC2, TC3, TC4 and TC4ELI, the thickness of the pure titanium or titanium alloy raw material coil is 1.5 mm to 5.0 mm, and the width of the strip after longitudinal shearing is 80 mm to 600 mm; The step 2 specifically includes: performing an "I"-shaped groove milling process at an angle of 30 to 100 degrees on the head (1) of the previous coil of strip and the tail (2) of the next coil of strip to expose a fresh metallic luster.

4. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that Specifically, the step 3 comprises: using a plasma arc welding method or a laser welding method to perform oblique butt welding of the strip to form an oblique butt weld (3); and simultaneously performing inert gas protection in a range of length×width=200 mm×20 mm near the high temperature area of ​​the front and back sides of the strip; The step 3 of performing seamless heat treatment on the weld specifically includes performing excess scraping treatment on the oblique butt weld (3) using a high temperature resistant and sticking resistant hard alloy scraper and performing vacuum seamless heat treatment on the oblique weld using a linear special heat treatment device, so as to ensure that the weld is flat and the structure is consistent with that of the parent material; The vacuum seamless heat treatment process of the weld is: firstly rapidly heated to 950°C~1000°C for heat treatment, kept at this temperature for 30s~120s and then cooled to room temperature with water, then rapidly heated to 550°C~650°C, kept at this temperature for 30s~120s and then naturally cooled to room temperature; The step 4 specifically includes: using a special tool to continuously perform "I"-shaped groove milling on both longitudinal sides of the pure titanium or titanium alloy strip online, without edge wrinkles and defects; and using laser impact shot peening technology to perform nano-treatment on the outer surface of the pure titanium or titanium alloy strip, with a coverage rate of 100%.

5. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that The step 5 is specifically as follows: firstly, the two longitudinal edges of the strip are continuously bent and formed by the first set of special rollers, then the strip is continuously bent and deformed from the edge to the inside by the subsequent special rollers, and finally, an external special roller pair is used to extrude and form the strip from the outside into a tube.

6. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that The step 6 is specifically as follows: a plasma arc welding method or a laser welding method is used to perform continuous longitudinal seam welding at the joint point to form a longitudinal weld of the pure titanium or titanium alloy pipe, the groove gap at the joint point is 0, the lateral extrusion amount is 0.3mm~1.0mm, and inert gas protection is simultaneously performed within a range of length×width=200mm×20mm near the high temperature zone of the inner and outer welds of the pipe.

7. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that The step 7 is specifically as follows: using a high temperature resistant and sticky resistant carbide scraper to continuously scrape the longitudinal seam excess height, and the seamless heat treatment process is specifically as follows: first rapidly heat to 950°C~1000°C for heat treatment, keep warm for 30s~120s and then cool to room temperature with water, then rapidly heat to 550°C~650°C, keep warm for 30s~120s and then naturally cool to room temperature.

8. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that The temperature monitoring sensor (6), the wall thickness monitoring sensor (7) and the pressure monitoring sensor (8) in step 8 are evenly arranged in sequence at equal angles along the circumference of the pipe body; The thickness of the carbon fiber layer (9) in step 9 is 1 mm to 4 mm.

9. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that In the step 10, a liquid resin solution is used for impregnation treatment, the impregnation temperature is 50° C. to 250° C., and the impregnation time is 30s to 300s. The curing treatment adopts a linear continuous curing treatment device.

10. The method for producing a pure titanium or titanium alloy composite continuous pipe according to claim 2, It is characterized in that The prepared carbon fiber-coated pure titanium or titanium alloy composite continuous tube is continuously wound on a reel device with a diameter of 800mm~2000mm. The end of the tube is locked with the reel outer frame device with a special lock, and the port is protected with a sealing ring.

Citation Information

Patent Citations

  • Compound pipe production method based on spraying technology

    CN113458549A

  • Production and preparation method of pure titanium or titanium alloy continuous pipe

    CN114523271A

  • Manufacturing method of composite material continuous gathering and transportation pipe

    CN116968359A

  • Monitoring device and monitoring method for composite material reinforced pipeline based on optical fiber

    CN117249765A

  • High-performance, corrosion-resistant and economical composite steel coiled tubing and manufacturing method therefor