Multi-dimensional disordered rock salt, composite material as well as preparation method and application of multi-dimensional disordered rock salt and composite material
By crosslinking multi-dimensional disordered rock salt with conductive carbon-based materials to form composite electrodes, and coating them with non-conductive polymers to form composite solid electrolytes, the problems of easy collapse of the negative electrode material structure of lithium-ion batteries and poor performance of solid electrolytes are solved, and the problem of poor performance of solid electrolytes is achieved. Efficient lithium ion transmission and battery cycle stability improve battery safety and energy density.
Patent Information
- Application Number
- CN202411093835.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-29
AI Technical Summary
The negative electrode material structure of existing lithium-ion batteries is prone to collapse, resulting in a shortening of cycle life, and the conductivity and mechanical properties of solid electrolytes are poor, which cannot meet the high lithium ion migration number and high Young's modulus at the same time, which poses safety risks.
Multi-dimensional disordered rock salt material is cross-linked with conductive carbon-based materials to form composite electrodes, and composite solid electrolytes are formed by coating non-conductive polymers, providing additional lithium ion transmission paths, improving conductivity and mechanical properties, and reducing the crushing of active materials. and fall off.
It significantly improves the transmission efficiency of lithium ions and the cycle stability of the battery, enhances electrochemical and mechanical properties, extends the battery life, and improves safety, meeting the needs of high energy density and high power density.
Smart Images

Figure CN119038601A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical energy storage devices, and in particular to a multi-dimensional disordered rock salt, a composite material, and a preparation method and application thereof. Background Art
[0002] Lithium batteries are one of the representatives of advanced electrochemical storage and conversion devices. With the increasing demand for high-performance batteries in diversified energy storage applications, lithium-ion batteries must not only meet the requirements of low cost and safety, but also meet the performance requirements of high energy density, high power density and long cycle life. However, graphite-based lithium-ion batteries are limited by the low capacity of the negative electrode (372mAh g -1 ), the layered graphite structure is prone to collapse as the number of lithium ion insertion / extraction cycles increases, resulting in a shortened battery cycle life, and severe polarization can easily lead to safety hazards. In addition, commercial lithium-ion batteries currently mainly use organic electrolytes, which have safety hazards such as leakage, combustion, and explosion in unconventional environments.
[0003] To date, a lot of work has been done on the search and development of negative electrode materials and electrolytes for lithium batteries. Lithium-rich disordered rock salt-rich oxides and / or fluorine-containing oxides are considered to be promising negative electrode materials for lithium batteries due to their safe insertion potential, higher theoretical capacity relative to graphite, and fast lithium ion transport. However, they face great challenges due to poor conductivity and complex percolation networks at multiple scales. To address these obstacles, many efforts have focused on adding large amounts of conductive agents or adjusting the structure and doping engineering to improve ionic and electronic conductivity. These efforts include using fluorinated electrolytes to improve ion transport by forming a low-resistance LiF-rich solid electrolyte interface (SEI) layer, reducing particle size, or pre-inserting polyaniline into Li + Doping is combined with the expansion of the Li-embedded layer. This strategy can reduce the lithium-ion diffusion barrier, but the energy density of the device is inevitably sacrificed due to the incorporation of inert components (binders or polymers). Solid electrolytes can be divided into inorganic electrolytes and polymer electrolytes. In terms of inorganic solid electrolytes, the garnet structure lithium-ion solid electrolyte (Li7La3Zr2O 12 , LLZO) has high conductivity (~10 -3 S cm -1 ), wide electrochemical window (0-4V), etc., and is one of the candidate electrolyte materials for the next generation of high-safety solid-state lithium batteries. However, its high sintering temperature, usually above 1100°C, and its fragile nature and high interface resistance greatly hinder its practical application. In addition, solid polymer electrolytes, such as polyphenylene ether and polyethylene oxide (PEO), can be easily processed. However, the electrochemical and mechanical properties of pure polymer electrolytes are not ideal, and the room temperature ionic conductivity is usually very low (10-5 -10 -10 S cm -1 ), the electrochemical window is generally lower than 3.8 V, and their Young's modulus is generally very low, lower than 0.4 MPa, which is difficult to meet the growing demand in practical applications.
[0004] In response to the above problems, the current solutions mainly focus on the following aspects: 1. It is necessary to improve the ability of the electrode to transfer electrons and ions in a coordinated manner and increase its chemical and mechanical stability. The current electrodes are all doped with inert components (binders or polymers), which inevitably increases the internal resistance of the electrode and reduces the energy density of the electrode; 2. Solid electrolytes cannot simultaneously meet high lithium ion migration numbers and ionic conductivity, and have a low Young's modulus, which cannot effectively inhibit the growth of lithium dendrites. Summary of the invention
[0005] The purpose of the present invention is to provide a multidimensional disordered rock salt, a composite material and a preparation method and application thereof in order to overcome the defects of the above-mentioned prior art, and to use the unique structure and chemical properties of the multidimensional disordered rock salt material to optimize the performance of electrochemical energy storage devices, improve energy density and cycle stability, explore new material systems, solve resource sustainability problems, and improve battery safety. The multidimensional disordered rock salt material and the conductive carbon-based material are cross-linked to form a strong, binder-free, flexible self-supporting multidimensional disordered rock salt composite electrode, which can increase the conductivity and accelerate the transmission of lithium ions on the one hand; on the other hand, it can show excellent mechanical properties and reduce the breakage and shedding of active materials. The multidimensional disordered rock salt material is coated with a non-conductive polymer to become a multidimensional disordered rock salt composite solid electrolyte, in which the multidimensional disordered rock salt composite electrode provides an additional lithium ion transmission path as an active filler, thereby significantly improving the ionic conductivity of the multidimensional disordered rock salt composite solid electrolyte. After the active filler is composited with the polymer, lithium ions can be conducted at the organic phase, inorganic phase and the interface between the two phases, improving the overall performance of the multidimensional disordered rock salt composite solid electrolyte.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a multi-dimensional disordered rock salt material, wherein the disordered rock salt material is a lithium-rich transition metal oxide, and its general formula is: Li x M y O z , 0<x≤5, y>0, z>0, M includes one or more of chromium (Cr), vanadium (V), molybdenum (Mo), titanium (Ti), niobium (Nb), manganese (Mn), zirconium (Zr), nickel (Ni), iron (Fe), ruthenium (Ru), copper (Cu), magnesium (Mg), tungsten (W), and tantalum (Ta);
[0008] The disordered rock salt material is a one-dimensional disordered rock salt nanowire or a two-dimensional disordered rock salt nanosheet.
[0009] Furthermore, the lithium-rich transition metal oxide includes a fluorine-containing lithium-rich transition metal oxide, and the general formula of the fluorine-containing lithium-rich transition metal oxide is: Li a M' b O c F d , 0<a≤5; 0<b≤1; 0<c≤2; 0<d≤2; M' includes one or more of chromium Cr, V, Mo, Ti, Nb, Mn, Zr, Ni, Fe, Ru, Cu, Mg, W, and Ta.
[0010] The second technical solution of the present invention is to provide a method for preparing a multi-dimensional disordered rock salt material, including an in-situ electrochemical lithiation method or a chemical lithiation method;
[0011] The in-situ electrochemical lithiation method is as follows: assembling a one-dimensional or two-dimensional transition metal oxide into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the transition metal oxide under the action of an electric field to obtain a multi-dimensional disordered rock salt material;
[0012] The chemical lithiation method is as follows: a strongly reducing lithium-containing reagent undergoes an oxidation-reduction reaction with a one-dimensional or two-dimensional transition metal oxide to transfer active lithium to the transition metal oxide to obtain a multi-dimensional disordered rock salt material.
[0013] Furthermore, the one-dimensional or two-dimensional transition metal oxide is assembled into a half-cell, and a lithium-containing electrolyte is used to discharge from an open circuit voltage to 0.01 to 0.05 V at 0.05 to 0.5 A·g -1 The current density is charged to 2.4-2.6V, and the lithium ions are embedded in the transition metal oxide under the action of the electric field, thereby synthesizing multi-dimensional disordered rock salt materials.
[0014] The transition metal oxide includes one or more of TiO2, V2O5, Nb2O5, MoO3, ZrO2, MnO, Mn2O3, NiO, Ni2O3, FeO and Fe2O3,
[0015] The half-cell further includes a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the one-dimensional or two-dimensional transition metal oxide is located between the gasket and the electrolyte;
[0016] The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate;
[0017] The molar ratio of the transition metal oxide to the lithium-containing electrolyte is 1:(1-2);
[0018] In the chemical lithiation method:
[0019] The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution;
[0020] The molar ratio of the transition metal oxide to the lithium-containing solution is 1:(3-4).
[0021] The third technical solution of the present invention is to provide a multi-dimensional disordered rock salt composite material, comprising the above-mentioned multi-dimensional disordered rock salt material, and also comprising a conductive carbon-based material or a non-conductive polymer;
[0022] The multidimensional disordered rock salt material and the conductive carbon-based material are cross-linked with each other to obtain a multidimensional disordered rock salt composite electrode with a self-supporting structure, wherein the conductive carbon-based material serves as a conductive material and the multidimensional disordered rock salt material serves as an active substance; wherein the conductive carbon-based material serves to support the structure and provide an electron conduction path, and the multidimensional disordered rock salt material serves to provide storage sites for lithium ions and improve the transmission kinetics of lithium ions.
[0023] The non-conductive polymer wraps the multi-dimensional disordered rock salt material to obtain a multi-dimensional disordered rock salt composite solid electrolyte, wherein the disordered rock salt composite electrode serves as an active filler and the non-conductive polymer serves as a substrate.
[0024] Further, the conductive carbon-based material includes carbon nanotubes, graphene, activated carbon or MXene;
[0025] The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the conductive carbon-based material is 5% to 35%;
[0026] The non-conductive polymer includes polyvinyl acrylate, polyvinylene carbonate, and polyacrylonitrile;
[0027] The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the non-conductive polymer is 5% to 35%.
[0028] The fourth technical solution of the present invention is to provide a method for preparing a multidimensional disordered rock salt composite material. The preparation process of the multidimensional disordered rock salt composite electrode is as follows: a transition metal oxide precursor, a template, a conductive carbon-based material and a solvent are mixed and then subjected to a hydrothermal reaction, and after the reaction is completed, lithium is formed to obtain a multidimensional disordered rock salt composite electrode;
[0029] The preparation process of the multidimensional disordered rock salt composite solid electrolyte is as follows: a non-conductive polymer is poured onto the multidimensional disordered rock salt material, and an in-situ polymerization reaction is performed to obtain a multidimensional disordered rock salt composite solid electrolyte.
[0030] Furthermore, in the preparation process of the multi-dimensional disordered rock salt composite electrode:
[0031] The multi-dimensional disordered rock salt composite electrode comprises 0.5% to 2% by mass of a transition metal oxide precursor, 1% to 5% by mass of a template, 0.1% to 0.5% by mass of a conductive carbon-based material, and 95% to 98% by mass of a solvent.
[0032] The transition metal oxide precursor includes ammonium metavanadate, ammonium metatungstate, ammonium metamolybdate, potassium vanadate or sodium vanadate.
[0033] The template agent includes polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, tetrapropylammonium hydroxide, citric acid, polyvinyl alcohol or polyethylene glycol,
[0034] The solvent is water,
[0035] The temperature of the hydrothermal reaction is 100-300°C.
[0036] The lithiation method is an in-situ electrochemical lithiation method or a chemical lithiation method.
[0037] The mixing is performed by stirring and mixing for 12 to 48 hours;
[0038] The conductive carbon-based material is subjected to modification and acidification treatment before mixing.
[0039] Furthermore, the conductive carbon-based material is modified and acidified, and the specific process is: mixing the conductive carbon-based material, concentrated nitric acid and concentrated sulfuric acid, stirring, filtering, vacuum drying, and high-speed shear dispersion.
[0040] Furthermore, the specific process of the in-situ electrochemical lithiation method is: assembling the disordered rock salt composite material into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the disordered rock salt-based composite material under the action of an electric field to obtain a disordered rock salt composite electrode;
[0041] The half-cell further comprises a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the disordered rock salt-based composite material is located between the gasket and the electrolyte;
[0042] The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate;
[0043] The molar ratio of the disordered rock salt-based composite material to the lithium-containing electrolyte is 1:(1-2);
[0044] The specific process of the chemical lithiation method is: mixing the disordered rock salt-based composite material with a strong reducing lithium-containing reagent under an inert atmosphere to obtain a disordered rock salt composite electrode;
[0045] The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution;
[0046] The molar ratio of the disordered rock salt-based composite material to the lithium-containing solution is 1:(3-4).
[0047] Furthermore, during the modification and acidification process of the conductive carbon-based material, the stirring time is 30 to 80 minutes, the vacuum drying temperature is 60 to 100° C., the time is 6 to 24 hours, and the high-speed shear dispersion time is 10 to 60 seconds.
[0048] Furthermore, the preparation process of the multidimensional disordered rock salt composite electrode is: mixing transition metal oxides, templates, conductive carbon-based materials and solvents, hydrothermally reacting, washing, drying and then filtering to form a film, and lithiation the membrane to obtain a multidimensional disordered rock salt composite electrode.
[0049] Furthermore, the multi-dimensional disordered rock salt material contained in the multi-dimensional disordered rock salt composite material can also be a three-dimensional structure.
[0050] Furthermore, the preparation process of the multi-dimensional disordered rock salt composite solid electrolyte is as follows:
[0051] The temperature of the in-situ polymerization reaction is 60-90°C, preferably 70-80°C.
[0052] Furthermore, the non-conductive polymer comprises 0.5% to 2% by mass of a monomer, 1% to 5% by mass of a cross-linking agent, 0.1% to 0.5% by mass of a lithium salt, and 95% to 98% by mass of an initiator.
[0053] Furthermore, the monomers include vinyl acrylate and vinylene carbonate;
[0054] The cross-linking agent includes ethylene glycol dimethacrylate and pentaerythritol tetraacrylate;
[0055] The lithium salts include lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium perchlorate, and lithium dioxalatoborate;
[0056] The initiator includes azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0057] Furthermore, the preparation process of the non-conductive polymer is: the monomer, the cross-linking agent, the lithium salt and the initiator are uniformly mixed at a temperature of 40 to 80° C. to obtain the non-conductive polymer.
[0058] The fifth technical solution of the present invention is to provide an application of a multi-dimensional disordered rock salt composite material in the field of electrochemical energy storage devices, wherein the electrochemical energy storage devices include lithium metal batteries, lithium ion batteries, supercapacitors, lithium air batteries, and solid electrolytes.
[0059] Compared with the prior art, the present invention has the following advantages:
[0060] (1) In the structure of the one-dimensional disordered rock salt material of the present invention, lithium ions and transition metal cations are disorderly arranged at the cation position, and the structure is more stable. The unit cell parameters of the rock salt structure are small, and Li + An activated tetrahedral site diffuses through two adjacent octahedral sites, and there are no coplanar TM cations in the diffusion path, forming a so-called 0-TM channel.
[0061] (2) In the multi-dimensional disordered rock salt composite electrode prepared by the present invention, the conductive carbon-based material provides a fast electron transmission pathway, and the multi-dimensional disordered rock salt material structure can effectively realize the coordinated transfer of electrons and ions by shortening the diffusion distance of lithium ions.
[0062] (3) The one-dimensional disordered rock salt composite electrode of the present invention has an interwoven three-dimensional network structure, which creates interconnected channels for effective ion transport. At the same time, this interpenetrating network enables the electrode to have excellent mechanical properties and high-rate lithium storage performance.
[0063] (4) The two-dimensional disordered rock salt composite electrode of the present invention is composed of optimized vertically aligned channels composed of 2D heterostructures, which continuously provide better performance with increasing mass loading compared to the commonly used horizontally stacked electrodes. On the one hand, the two-dimensional heterostructures stacked in a "sheet-to-sheet" manner promote electron transport, buffer volume expansion, and avoid the use of inactive agents (metal current collectors, conductive additives, and polymer binders). On the other hand, the vertical channels provide a path for the rapid transport of electrons / ions throughout the electrode. Both of these characteristics ensure fast charge / discharge capabilities and good cycle stability.
[0064] (5) The multi-dimensional disordered rock salt composite electrode prepared by the present invention has excellent mechanical properties. The rigid-flexible interface can effectively prevent electrode deactivation and aggregation of active particles in the absence of a continuous conductive network, thereby ensuring the stability of the conductive network and mechanical network of the composite electrode.
[0065] (6) The multi-dimensional disordered rock salt composite electrode prepared by the present invention mainly forms a self-supporting film by entanglement between the multi-dimensional disordered rock salt material and the conductive carbon-based material, does not require a binder and a current collector, and improves the energy density of the entire battery.
[0066] (7) The multi-dimensional disordered rock salt composite electrode prepared by the present invention has a hierarchical porous structure, which provides high electrolyte absorption, fast lithium diffusion and kinetics. In addition to the nanowires with short ion diffusion length, the lithiation-driven process also retains the interconnected channels of the scaffold to facilitate lithium ion transport.
[0067] (8) The multidimensional disordered rock salt composite electrode prepared by the present invention has high capacity, high initial coulombic efficiency, excellent rate performance, and long cycle life. The further constructed full battery has high mass energy density and high volume energy density.
[0068] (9) The multidimensional disordered rock salt composite solid electrolyte prepared by the present invention, wherein the multidimensional disordered rock salt material is used as an active filler to provide an additional lithium ion transmission path, thereby significantly improving the ion migration number and conductivity of the composite solid electrolyte. After the active filler is composited with the polymer, lithium ions can be conducted in the organic phase, the inorganic phase and the interface between the two phases, thereby improving the overall performance of the solid electrolyte.
[0069] (10) The multi-dimensional disordered rock salt composite solid electrolyte prepared by the present invention has excellent electrochemical stability and mechanical strength, and can resist lithium dendrite cycling, thereby improving safety. It provides innovative insights for the development of high-area capacity and long-life lithium batteries, and provides a promising path for high-performance lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 This is the SEM image of LVO / CNT prepared in Example 1;
[0071] Figure 2 TEM image of LVO / CNT prepared in Example 1;
[0072] Figure 3 A comparison chart of the rate performance of LVO / CNT prepared in Example 1 and Bulk-LVO prepared in Comparative Example 1 as negative electrode materials for lithium-ion batteries at different current densities;
[0073] Figure 4 A comparison of the cycle stability of LVO / CNT prepared in Example 1 and Bulk-LVO prepared in Comparative Example 1 as negative electrode materials for lithium-ion batteries at 2C; a cycle stability diagram of LVO / CNT as negative electrode materials for lithium-ion batteries at 1C;
[0074] Figure 5This is a comparison chart of the rate performance of LSPE prepared in Example 2 as a composite polymer solid electrolyte for lithium-ion batteries at different current densities;
[0075] Figure 6 A comparison chart of the cycle stability of the LSPE prepared in Example 2 and the SPE prepared in Comparative Example 2 as composite polymer solid electrolytes for lithium-ion batteries at a rate of 0.5C;
[0076] Figure 7 A comparison chart of the cycle stability of the LSPE prepared in Example 2 and the SPE prepared in Comparative Example 2 as composite polymer solid electrolytes for lithium-ion batteries at a rate of 1C;
[0077] Figure 8 The ratio of the surface capacity of LVO / MXene prepared in Example 3 to other reported negative electrode materials at different current densities. DETAILED DESCRIPTION
[0078] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the given embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0079] A multi-dimensional disordered rock salt material, wherein the disordered rock salt material is a lithium-rich transition metal oxide, and its general formula is: Li x M y O z , 0<x≤5, y>0, z>0, M includes one or more of chromium (Cr), vanadium (V), molybdenum (Mo), titanium (Ti), niobium (Nb), manganese (Mn), zirconium (Zr), nickel (Ni), iron (Fe), ruthenium (Ru), copper (Cu), magnesium (Mg), tungsten (W), and tantalum (Ta);
[0080] The disordered rock salt material is a one-dimensional disordered rock salt nanowire or a two-dimensional disordered rock salt nanosheet.
[0081] As one of the preferred embodiments, the lithium-rich transition metal oxide includes a fluorine-containing lithium-rich transition metal oxide, and the general formula of the fluorine-containing lithium-rich transition metal oxide is: Li a M' b O c F d , 0<a≤5; 0<b≤1; 0<c≤2; 0<d≤2; M' includes one or more of chromium Cr, V, Mo, Ti, Nb, Mn, Zr, Ni, Fe, Ru, Cu, Mg, W, and Ta.
[0082] A method for preparing a multi-dimensional disordered rock salt material, comprising an in-situ electrochemical lithiation method or a chemical lithiation method;
[0083] The in-situ electrochemical lithiation method is as follows: assembling a one-dimensional or two-dimensional transition metal oxide into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the transition metal oxide under the action of an electric field to obtain a multi-dimensional disordered rock salt material;
[0084] The chemical lithiation method is as follows: a strongly reducing lithium-containing reagent undergoes an oxidation-reduction reaction with a one-dimensional or two-dimensional transition metal oxide to transfer active lithium to the transition metal oxide to obtain a multi-dimensional disordered rock salt material.
[0085] As one of the preferred embodiments, a one-dimensional or two-dimensional transition metal oxide is assembled into a half-cell, and a lithium-containing electrolyte is used to discharge from an open circuit voltage to 0.01 to 0.05 V at 0.05 to 0.5 A·g -1 The current density is charged to 2.4-2.6V, and the lithium ions are embedded in the transition metal oxide under the action of the electric field, thereby synthesizing multi-dimensional disordered rock salt materials.
[0086] The transition metal oxide includes one or more of TiO2, V2O5, Nb2O5, MoO3, ZrO2, MnO, Mn2O3, NiO, Ni2O3, FeO and Fe2O3,
[0087] The half-cell further includes a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the one-dimensional or two-dimensional transition metal oxide is located between the gasket and the electrolyte;
[0088] The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate;
[0089] The molar ratio of the transition metal oxide to the lithium-containing electrolyte is 1:(1-2);
[0090] In the chemical lithiation method:
[0091] The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution;
[0092] The molar ratio of the transition metal oxide to the lithium-containing solution is 1:(3-4).
[0093] A multi-dimensional disordered rock salt composite material, comprising the above-mentioned multi-dimensional disordered rock salt material, and also comprising a conductive carbon-based material or a non-conductive polymer;
[0094] The multidimensional disordered rock salt material and the conductive carbon-based material are cross-linked with each other to obtain a multidimensional disordered rock salt composite electrode with a self-supporting structure, wherein the conductive carbon-based material serves as a conductive material and the multidimensional disordered rock salt material serves as an active substance; wherein the conductive carbon-based material serves to support the structure and provide an electron conduction path, and the multidimensional disordered rock salt material serves to provide storage sites for lithium ions and improve the transmission kinetics of lithium ions.
[0095] The non-conductive polymer wraps the multi-dimensional disordered rock salt material to obtain a multi-dimensional disordered rock salt composite solid electrolyte, wherein the disordered rock salt composite electrode serves as an active filler and the non-conductive polymer serves as a substrate.
[0096] As one of the preferred embodiments, the conductive carbon-based material includes carbon nanotubes, graphene, activated carbon or MXene;
[0097] The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the conductive carbon-based material is 5% to 35%;
[0098] The non-conductive polymer includes polyvinyl acrylate, polyvinylene carbonate, and polyacrylonitrile;
[0099] The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the non-conductive polymer is 5% to 35%.
[0100] A method for preparing a multidimensional disordered rock salt composite material, wherein the preparation process of the multidimensional disordered rock salt composite electrode is as follows: a transition metal oxide precursor, a template agent, a conductive carbon-based material and a solvent are mixed and then subjected to a hydrothermal reaction, and after the reaction is completed, lithium is carried out to obtain a multidimensional disordered rock salt composite electrode;
[0101] The preparation process of the multidimensional disordered rock salt composite solid electrolyte is as follows: a non-conductive polymer is poured onto the multidimensional disordered rock salt material, and an in-situ polymerization reaction is performed to obtain a multidimensional disordered rock salt composite solid electrolyte.
[0102] As one of the preferred embodiments, during the preparation of the multi-dimensional disordered rock salt composite electrode:
[0103] The multi-dimensional disordered rock salt composite electrode comprises 0.5% to 2% by mass of a transition metal oxide precursor, 1% to 5% by mass of a template, 0.1% to 0.5% by mass of a conductive carbon-based material, and 95% to 98% by mass of a solvent.
[0104] The transition metal oxide precursor includes ammonium metavanadate, ammonium metatungstate, ammonium metamolybdate, potassium vanadate or sodium vanadate.
[0105] The template agent includes polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, tetrapropylammonium hydroxide, citric acid, polyvinyl alcohol or polyethylene glycol,
[0106] The solvent is water,
[0107] The temperature of the hydrothermal reaction is 100-300°C.
[0108] The lithiation method is an in-situ electrochemical lithiation method or a chemical lithiation method.
[0109] The mixing is performed by stirring and mixing for 12 to 48 hours;
[0110] The conductive carbon-based material is subjected to modification and acidification treatment before mixing.
[0111] As one of the preferred implementations, the conductive carbon-based material is modified and acidified, and the specific process is: mixing the conductive carbon-based material, concentrated nitric acid and concentrated sulfuric acid, stirring, filtering, vacuum drying, and high-speed shear dispersion.
[0112] As one of the preferred embodiments, the specific process of the in-situ electrochemical lithiation method is: assembling the disordered rock salt composite material into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the disordered rock salt-based composite material under the action of an electric field to obtain a disordered rock salt composite electrode;
[0113] The half-cell further comprises a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the disordered rock salt-based composite material is located between the gasket and the electrolyte;
[0114] The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate;
[0115] The molar ratio of the disordered rock salt-based composite material to the lithium-containing electrolyte is 1:(1-2);
[0116] The specific process of the chemical lithiation method is: mixing the disordered rock salt-based composite material with a strong reducing lithium-containing reagent under an inert atmosphere to obtain a disordered rock salt composite electrode;
[0117] The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution;
[0118] The molar ratio of the disordered rock salt-based composite material to the lithium-containing solution is 1:(3-4).
[0119] As one of the preferred implementations, during the modification and acidification process of the conductive carbon-based material, the stirring time is 30 to 80 minutes, the vacuum drying temperature is 60 to 100° C., the time is 6 to 24 hours, and the high-speed shear dispersion time is 10 to 60 seconds.
[0120] As one of the preferred embodiments, the preparation process of the multidimensional disordered rock salt composite electrode is: mixing and stirring transition metal oxides, templates, conductive carbon-based materials and solvents, hydrothermally reacting, washing, drying and then filtering to form a film, and lithiation the membrane to obtain a multidimensional disordered rock salt composite electrode.
[0121] The multi-dimensional disordered rock salt material contained in the multi-dimensional disordered rock salt composite material may have a three-dimensional structure in addition to a one-dimensional or two-dimensional structure.
[0122] As one of the preferred embodiments, the preparation process of the multi-dimensional disordered rock salt composite solid electrolyte is as follows:
[0123] The temperature of the in-situ polymerization reaction is 60-90°C, preferably 70-80°C.
[0124] As one of the preferred embodiments, the non-conductive polymer includes 0.5% to 2% by mass of monomers, 1% to 5% by mass of cross-linking agent, 0.1% to 0.5% by mass of lithium salt, and 95% to 98% by mass of initiator.
[0125] As one of the preferred embodiments, the monomers include vinyl acrylate and vinylene carbonate;
[0126] The cross-linking agent includes ethylene glycol dimethacrylate and pentaerythritol tetraacrylate;
[0127] The lithium salts include lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium perchlorate, and lithium dioxalatoborate;
[0128] The initiator includes azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.
[0129] As one of the preferred implementations, the preparation process of the non-conductive polymer is: monomers, cross-linking agents, lithium salts, and initiators are uniformly mixed at a temperature of 40 to 80° C. to obtain the non-conductive polymer.
[0130] An application of a multi-dimensional disordered rock salt composite material in the field of electrochemical energy storage devices, wherein the electrochemical energy storage devices include lithium metal batteries, lithium ion batteries, supercapacitors, lithium air batteries, and solid electrolytes.
[0131] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art.
[0132] In the following embodiments, the test methods used are as follows:
[0133] Field emission scanning electron microscope (SEM) test, using JSM-7800F equipment model. The disordered rock salt-based composite material was adhered to the conductive adhesive, and then gold was sprayed for 15s to improve the conductivity of the material, and its surface morphology was observed.
[0134] Transmission electron microscopy (TEM) was performed using the American Thermo Fisher FEI Talos F200s equipment model. The disordered rock salt-based composite material was ultrasonically dispersed with ethanol to observe its surface morphology.
[0135] Electrochemical testing:
[0136] Constant current charge and discharge method (GC): Constant current charge and discharge method is an important method for studying electrochemical properties. Its working principle is mainly to check the charging and discharging process of various electrodes under constant current conditions, record the changes of different power levels of electrodes over time, and determine a series of parameters such as specific capacity, coulomb efficiency, energy efficiency, etc. by analyzing and studying the charging and discharging characteristics of various electrodes, so as to judge the electrochemical performance of materials. The constant current charge and discharge test was carried out using Wuhan Blue Electric CT2001A battery test system.
[0137] In the following embodiments, the polyvinylidene fluoride (PVDF) has a CAS number of 24937-79-9, an average Mw of 534,000 by GPC, powder, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; the multi-walled carbon nanotubes (CNTs) have a CAS number of 1333-86-4, a purity of 98%, and a length of 0.5-2 microns, purchased from Xianfeng Nanomaterial Technology Co., Ltd.; the CAS number of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) is 106392-12-5, an average Mw ~ 5,800, purchased from Sigma-Aldrich; vinyl acrylate CAS No. 105-38-4, purity 98%+, purchased from Adamas; ethylene glycol dimethacrylate CAS No. 97-90-5, purity 97%, purchased from TCl; lithium bis(trifluoromethanesulfonyl)imide CAS No. 90076-65-6, purity 98%+, purchased from Adamas; succinonitrile CAS No. 110-61 -2, purity 99%+, purchased from Adamas; the CAS number of azobisisobutyronitrile is 78-67-1, purity 98%+, purchased from Adamas, the CAS number of lithium nitrate is 7790-69-4, purity 99%+, purchased from Adamas; the CAS number of nickel carbonate is 3333-67-3, purity 98%, purchased from Alfa; the CAS number of lithium fluoride is 7789-24-4, purity 99.99%, purchased from Adamas.
[0138] Example 1
[0139] This embodiment provides a one-dimensional disordered rock salt composite electrode and a preparation method thereof, wherein the preparation process is as follows:
[0140] (1) In a 1L flask, add 12g of multi-walled CNTs and mix with 100mL of 65% concentrated nitric acid (HNO3) and 300mL of 98% concentrated sulfuric acid (H2SO4), and stir vigorously for acidification for 100 minutes while condensing and refluxing. Then, the reaction mixture is diluted with deionized water, filtered, and the upper filter residue is redispersed in water, and this process is repeated until the pH value of the filtrate is near neutral to obtain modified acidified multi-walled CNTs. Then, the modified acidified multi-walled CNTs are dried at 80℃ in a vacuum drying oven for 24h. Then, 10g of the dried modified acidified multi-walled CNTs are dispersed by a high-speed shearing machine for 70s, and the volume expands by about 250%. The dispersed multi-walled CNTs are dried at 80℃ for use.
[0141] (2) 0.25 g of surfactant P123 (EO 20 PO 70 EO 20, Ma=5800, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer) was dispersed in 15mL deionized water, and 0.078g of modified acidified multi-walled CNTs was added to the beaker and stirred and ultrasonicated for 24h; then, 0.5mL 2mol / L hydrochloric acid (HCl) and 0.15g ammonium metavanadate (NH4VO3) were slowly added in sequence, mixed under ultrasound for 10 minutes, and vigorously stirred for 24h, and then the mixture was transferred to a 50mL polytetrafluoroethylene hydrothermal reactor, and then the reactor was placed in a blast drying oven, heated to 120℃, and kept warm for 24h. The obtained precipitate was filtered and rinsed with water and acetone for many times, and the rinsed membrane was vacuum dried at 80℃ for 12h to obtain an intermediate, named one-dimensional V2O5 / CNT.
[0142] (3) A one-dimensional V2O5 / CNT with a thickness of 50 μm was directly assembled in a half-cell, where the electrode was a Li sheet (thickness: 1.0 mm, diameter: 15.8 mm) and the electrolyte was 1M LiPF6 (EC:DEC, v / v=1:1). The assembled half-electrode was discharged from the open circuit voltage to 0.01 V and then charged to 2.5 V at a current density of 0.1 A / g to prepare a one-dimensional disordered rock salt composite electrode through electrochemical lithiation, named LVO / CNT electrode, in which the mass fraction of LVO was 65% and the mass fraction of CNT was 35%.
[0143] Its SEM and TEM images are as follows Figure 1 and Figure 2 As shown, after deep lithiation, there is close contact between CNT and LVO nanowires.
[0144] Example 2
[0145] This embodiment provides a one-dimensional disordered rock salt composite solid electrolyte and a preparation method thereof (LSPE), and the preparation process is as follows:
[0146] (1) 0.15 g of vinyl acrylate monomer, 0.15 g of ethylene glycol dimethacrylate crosslinker, 0.3 g of lithium bis(trifluoromethanesulfonyl)imide, 0.5 g of succinonitrile solid crystal plasticizer, and 0.005 g of azobisisobutyronitrile initiator were premixed to form a uniform non-conductive polymer.
[0147] (2) 0.25 g of surfactant P123 was dispersed in 15 mL of deionized water; then, 0.5 mL of 2 mol / L hydrochloric acid (HCl) and 0.15 g of ammonium metavanadate (NH4VO3) were slowly added in sequence, mixed under ultrasound for 10 minutes, and stirred vigorously for 24 hours. The mixture was transferred to a 50 mL polytetrafluoroethylene hydrothermal reactor, and then the reactor was placed in a blast drying oven, heated to 120°C, and kept warm for 24 hours. The obtained precipitate was filtered and rinsed with water and acetone for several times, and the rinsed membrane was vacuum dried at 80°C for 12 hours to obtain a pure V2O5 nanowire membrane, i.e., a one-dimensional disordered rock salt material.
[0148] (3) The V2O5 nanowire film was punched into a small disc with a diameter of 16 mm. n-butyl lithium was used as a lithiation agent. The punched disc was immersed in a 1.2 M n-butyl lithium solution (the molar ratio of n-butyl lithium to V2O5 nanowire film was 3:1) for 2 hours. During the reaction, the color of the V2O5 nanowire film changed from green to black. After the reaction was completed, it was washed with n-hexane three times and dried in vacuum at room temperature for 10 minutes. The one-dimensional disordered rock salt material prepared by chemical lithiation was named DRS-Li x V2O5 nanowire film.
[0149] (4) Pour the polymer precursor solution evenly onto the DRS-Li x The V2O5 nanowire film was then placed on a glass plate and kept at 65°C for 24 hours to initiate polymerization to obtain a one-dimensional disordered rock salt composite solid electrolyte (LSPE) with a polymer mass fraction of 20%. x The mass fraction of V2O5 is 80%.
[0150] The composite solid electrolyte obtained above was assembled into button cells and electrochemical tests were performed.
[0151] Example 3
[0152] This embodiment provides a two-dimensional disordered rock salt composite electrode and a preparation method thereof, wherein the preparation process is as follows:
[0153] (1) Prepare an aqueous solution by dissolving 10 ml of 12 mol / L hydrochloric acid (HCl) and 1.4 g of lithium fluoride (LiF) in 10 ml of deionized water. Slowly mix 2.0 g of Ti3AlC2 powder with the LiF / HCl aqueous solution and stir continuously at 35 °C for 24 h. Then, wash the resulting product thoroughly 4-5 times until the pH value reaches 6, and re-ultrasonicate the product in 250 ml of deionized water for 1 hour. After the ultrasonication, centrifuge at 3500 rpm for 1 hour. Collect the supernatant containing well-dispersed MXene nanosheets.
[0154] (2) An aqueous dispersion was prepared by mixing 0.72 g of commercial V2O5 powder (Sigma-Aldrich) with 60 ml of deionized water. 5 ml of 30% H2O2 was slowly dripped into the V2O5 dispersion, and the mixed solution was stirred for 2 hours. When the color of the solution changed from brownish yellow to dark red, the mixed solution was immediately sealed and hydrothermally reacted at 190°C for 15 hours to form a brown V2O5 gel.
[0155] (3) The V2O5 gel and MXene suspension were mixed evenly, and the V2O5 content was controlled to be 60wt% and the concentration of the MXene / V2O5 mixed solution was maintained at 2mg / mL. Then, the obtained MXene / V2O5 homogeneous dispersion was freeze-dried overnight to obtain a vertically aligned MXene / V2O5 aerogel.
[0156] (4) The vertically oriented aerogel was mechanically punched and a 50 μm thick two-dimensional MXene / V2O5 was directly assembled in a half-cell, where the electrode was a Li sheet (thickness: 1.0 mm, diameter: 15.8 mm) and the electrolyte was 1M LiPF6 (EC:DEC, v / v=1:1). The assembled half-electrode was discharged from the open circuit voltage to 0.01 V and then charged to 2.5 V at a current density of 0.1 A / g to prepare a multidimensional disordered rock salt composite electrode through electrochemical lithiation, named LVO / MXene electrode.
[0157] The electrodes obtained above were assembled into button cells and electrochemical tests were performed.
[0158] Example 4
[0159] This embodiment provides a one-dimensional disordered rock salt composite electrode and a preparation method thereof. Compared with Embodiment 1, the difference is that the mass fraction of LVO is 95% and the mass fraction of CNT is 5%.
[0160] Example 5
[0161] This embodiment provides a one-dimensional disordered rock salt composite electrode and a preparation method thereof. Compared with Embodiment 1, the difference is that the mass fraction of LVO is 80% and the mass fraction of CNT is 20%.
[0162] Example 6
[0163] This embodiment provides a one-dimensional disordered rock salt composite solid electrolyte and a preparation method thereof. Compared with embodiment 2, the difference is that the mass fraction of the polymer is 35%, and DRS-Li x The mass fraction of V2O5 is 6%.
[0164] Example 7
[0165] This embodiment provides a one-dimensional disordered rock salt composite solid electrolyte and a preparation method thereof. Compared with embodiment 2, the difference is that the mass fraction of the polymer is 5%, and DRS-Li x The mass fraction of V2O5 is 95%.
[0166] Example 8
[0167] This embodiment provides a multi-dimensional disordered rock salt composite solid electrolyte and a preparation method thereof. Compared with Example 2, the difference is that the mass fraction of the polymer is 10%, and DRS-Li x The mass fraction of V2O5 is 90%.
[0168] Comparative Example 1
[0169] This comparative example provides a method for preparing powdered V2O5 as a negative electrode material for lithium-ion batteries (Bulk-LVO), and its application. The preparation process is as follows:
[0170] (1) 1.5 g of V2O5 powder (Sigma-Aldrich, >99.96%), 0.3 g of conductive carbon black (Super P) and 0.2 g of binder (PVDF) were weighed and ground into a uniform mixture using a mortar and a grinding rod. Then, the powder mixture was dispersed in an N-methylpyrrolidone solution and stirred at 1800 rpm for 2 h using a planetary stirrer.
[0171] (2) The electrode was coated on a copper foil (9 μm) using a scraper. The coated electrode was then vacuum dried at 80 °C for 12 h and cut into 12 mm electrode discs using a button cell slicer. The active material loading was approximately 2 mg cm -2 The electrodes and lithium sheets (0.45 μm) were assembled into a half-cell, which was charged at 0.1 Ag -1 The battery was discharged to 0.01 V at a current density of 0.1 V to obtain a lithium vanadate electrode (Bulk-LVO).
[0172] The electrodes obtained above were assembled into lithium ion half-cells, and electrochemical tests were performed using sodium perchlorate solution as electrolyte.
[0173] Comparative Example 2
[0174] This comparative example provides a polymer solid electrolyte (SPE) and a preparation method and application thereof, and the preparation process is as follows:
[0175] (1) 0.15 g of vinyl acrylate monomer, 0.15 g of ethylene glycol dimethacrylate crosslinker, 0.3 g of lithium bis(trifluoromethanesulfonyl)imide, 0.5 g of succinonitrile solid crystalline plasticizer, and 0.005 g of azobisisobutyronitrile initiator were premixed to form a uniform precursor solution.
[0176] (2) The precursor solution was cast onto a glass fiber support, which was then sandwiched between two pieces of stainless steel and heated at 65 °C for 24 h to initiate polymerization. The resulting polymer solid electrolyte was then peeled off the stainless steel.
[0177] The obtained polymer solid electrolyte was assembled into button cells and electrochemical tests were performed.
[0178] Figure 3 The rate performance comparison chart of LVO / CNT prepared in Example 1 and Bulk-LVO prepared in Comparative Example 1 as negative electrode materials for lithium-ion batteries at different rates (0.4, 0.8, 1.0, 2.0, 4.0C), where the horizontal axis is the number of cycles and the vertical axis is the capacity in grams (mAh g -1 ),Depend on Figure 3 It can be seen that DRS-Li x Lithium-ion batteries composed of V2O5 / CNT have better rate performance than Bulk-LVO.
[0179] Figure 4 This is a comparison chart of the cycle stability of LVO / CNT prepared in Example 1 and Bulk-LVO prepared in Comparative Example 1 as negative electrode materials for lithium-ion batteries at a 2C rate, where the abscissa is the number of cycles and the ordinate is the gram capacity (mAh g -1 ), the results show that LVO / CNT has higher capacity and cycle stability as lithium-ion battery anode compared with Bulk-LVO.
[0180] Figure 5 This is the rate performance diagram of the LSPE prepared in Example 2, where the horizontal axis is the number of cycles and the vertical axis is the capacity in grams (mAh g -1 ),Depend on Figure 5 It can be seen that even at 2C rate, the battery can provide 113.2mAh g -1 High specific capacity. Figure 6 and Figure 7 The LSPE prepared in Example 2 and the SPE prepared in Comparative Example 2 are compared in terms of cycle stability as solid electrolytes for lithium metal batteries at 0.5C and 1C rates, where the abscissa is the number of cycles and the ordinate is the capacity in grams (mAh g -1 ), the results show that LSPE has higher capacity and cycle stability than SPE as a solid electrolyte for lithium metal batteries.
[0181] Figure 8 The area capacity of LVO / MXene prepared in Example 3 and other reported electrodes (negative electrode materials) at different current densities are compared in detail in Table 1 below. Figure 8As shown in Table 1, the LVO / Mxene electrode with high loading outperforms other electrodes. -2 The current density of 1.58 mAh cm -2 High areal capacity even at 2.62 mA cm -2 At a current density of 1.12 mAh cm, the LVO / Mxene electrode still has a -2 The high areal capacity of LVO / Mxene electrodes demonstrates that they have great potential in practical applications.
[0182] Table 1 Area capacity of LVO / MXene prepared in Example 3 and other reported negative electrode materials at different current densities
[0183]
[0184] Reference 1: Wang H, Qin N, Li Y, Li Z, Zhang F, Luo W, Zeng C, Lu Z, Cheng H. Nafion as a facile binder additive stabilizes solid electrolyte interphaseon graphite anode. Carbon 2023; 205:435-43.
[0185] Reference 2: Zhang C, Dong L, Zheng N, Zhu H, Wu C, Zhao F, Liu W.Aligned graphene array anodes with dendrite-free behavior for high-performance Li-ionbatteries. Energy Storage Mater 2021;37:296-305.
[0186] Reference 3: Zhang Y, Huang J, Saito N, Yang X, Zhang Z, Yang L, HiranoSI. Layered Perovskite Lithium Yttrium Titanate as a Low-Potential and Ultrahigh-Rate Anode for Lithium-Ion Batteries. Adv Energy Mater 2022;12(31):2200922.
[0187] Reference 4: Wang Z, Yuan S, Tang X, Wang H, Zhang M, Liu F, Yao N, Ma Y. Enhanced Li-ion migration behavior in Li3V2O5 rock-salt anode via stepwise lattice tailoring. Energy Storage Mater 2023; 54: 284-93.
[0188] Reference 5: Liu H, Zhu Z, Yan Q, Yu S, He X, Chen Y, Zhang R, Ma L, Liu T, Li M, Lin R. A disordered rock salt anode for fast-charging lithium-ion batteries. Nature 2020; 585(7823): 63-7.
[0189] Reference 6: Zheng Z, Zao Y, Zhang Q, Cheng Y, Chen H, Zhang K, Wang M S, Peng D L. Robust erythrocyte-like Fe2O3@carbon with yolk-shell structures as high-performance anode for lithium ion batteries. Chem Eng J 2018; 347: 563-73. Reference 7: Yu W B, Hu Z Y, Jin J, Yi M, Yan M, Li Y, Wang H E, Gao H X, Mai L Q, Hasan T, Xu B X. Unprecedented and highly stable lithium storage capacity of (001) faceted nanosheet-constructed hierarchically porous TiO2 / rGO hybrid architecture for high-performance Li-ion batteries. Natl Sci Rev 2020; 7(6): 1046-58.
[0190] Reference 8: Xu C, Manukyan KV, Adams RA, Pol VG, Chen P, Varma A. One-step solution combustion synthesis of CuO / Cu2O / C anode for long cycle life Li-ionbatteries. Carbon 2019;142:51-9.
[0191] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A multidimensional disordered rock salt material, characterized in that: The disordered rock salt material is a lithium-rich transition metal oxide, and its general formula is: Li x M y O z , 0<x≤5, y>0, z>0, M includes one or more of Cr, V, Mo, Ti, Nb, Mn, Zr, Ni, Fe, Ru, Cu, Mg, W, Ta; The disordered rock salt material is a one-dimensional disordered rock salt nanowire or a two-dimensional disordered rock salt nanosheet.
2. A multi-dimensional disordered rock salt material according to claim 1, characterized in that: The lithium-rich transition metal oxide includes a fluorine-containing lithium-rich transition metal oxide, and the general formula of the fluorine-containing lithium-rich transition metal oxide is: Li a M' b O c F d , 0<a≤5; 0<b≤1; 0<c≤2; 0<d≤2; M' includes one or more of Cr, V, Mo, Ti, Nb, Mn, Zr, Ni, Fe, Ru, Cu, Mg, W, and Ta.
3. A method for preparing a multidimensional disordered rock salt material according to claim 1 or 2, characterized in that: Including in-situ electrochemical lithiation method or chemical lithiation method; The in-situ electrochemical lithiation method is as follows: assembling a one-dimensional or two-dimensional transition metal oxide into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the transition metal oxide under the action of an electric field to obtain a multi-dimensional disordered rock salt material; The chemical lithiation method is as follows: a strongly reducing lithium-containing reagent undergoes an oxidation-reduction reaction with a one-dimensional or two-dimensional transition metal oxide to transfer active lithium to the transition metal oxide to obtain a multi-dimensional disordered rock salt material.
4. The method for preparing a multi-dimensional disordered rock salt material according to claim 3, characterized in that: In the electrochemical lithiation method, a one-dimensional or two-dimensional transition metal oxide is assembled into a half-cell, and a lithium-containing electrolyte is used to discharge the half-cell from an open circuit voltage to 0.01 to 0.05 V at a rate of 0.05 to 0.5 A·g -1 The current density is charged to 2.4-2.6V, and the lithium ions are embedded in the transition metal oxide under the action of the electric field, thereby synthesizing multi-dimensional disordered rock salt materials. The transition metal oxide includes one or more of TiO2, V2O5, Nb2O5, MoO3, ZrO2, MnO, Mn2O3, NiO, Ni2O3, FeO and Fe2O3, The half-cell further includes a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the one-dimensional or two-dimensional transition metal oxide is located between the gasket and the electrolyte; The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate; The molar ratio of the transition metal oxide to the lithium-containing electrolyte is 1:(1-2); In the chemical lithiation method: The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution; The molar ratio of the transition metal oxide to the lithium-containing solution is 1:(3-4).
5. A multi-dimensional disordered rock salt composite material, characterized in that: A multidimensional disordered rock salt material comprising the multidimensional disordered rock salt material according to claim 1 or 2, and further comprising a conductive carbon-based material or a non-conductive polymer; The multi-dimensional disordered rock salt material and the conductive carbon-based material are cross-linked with each other to obtain a multi-dimensional disordered rock salt composite electrode with a self-supporting structure, wherein the conductive carbon-based material serves as a conductive material and the multi-dimensional disordered rock salt material serves as an active material; The non-conductive polymer wraps the multi-dimensional disordered rock salt material to obtain a multi-dimensional disordered rock salt composite solid electrolyte, wherein the disordered rock salt composite electrode serves as an active filler and the non-conductive polymer serves as a substrate.
6. The multi-dimensional disordered rock salt composite material according to claim 5, characterized in that: The conductive carbon-based material includes carbon nanotubes, graphene, activated carbon or MXene; The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the conductive carbon-based material is 5% to 35%; The non-conductive polymer includes polyvinyl acrylate, polyvinylene carbonate, and polyacrylonitrile; The mass fraction of the multi-dimensional disordered rock salt material in the multi-dimensional disordered rock salt composite material is 65% to 95%, and the mass fraction of the non-conductive polymer is 5% to 35%.
7. A method for preparing a multi-dimensional disordered rock salt composite material according to claim 6, characterized in that: The preparation process of the multi-dimensional disordered rock salt composite electrode is as follows: a transition metal oxide precursor, a template agent, a conductive carbon-based material and a solvent are mixed and then subjected to a hydrothermal reaction, and after the reaction is completed, lithium is carried out to obtain a multi-dimensional disordered rock salt composite electrode; The preparation process of the multidimensional disordered rock salt composite solid electrolyte is as follows: a non-conductive polymer is poured onto the multidimensional disordered rock salt material, and an in-situ polymerization reaction is performed to obtain a multidimensional disordered rock salt composite solid electrolyte.
8. The method for preparing a multi-dimensional disordered rock salt composite material according to claim 7, characterized in that: In the preparation process of the multi-dimensional disordered rock salt composite electrode: The multi-dimensional disordered rock salt composite electrode comprises 0.5% to 2% by mass of a transition metal oxide precursor, 1% to 5% by mass of a template, 0.1% to 0.5% by mass of a conductive carbon-based material, and 95% to 98% by mass of a solvent. The transition metal oxide precursor includes ammonium metavanadate, ammonium metatungstate, ammonium metamolybdate, potassium vanadate or sodium vanadate. The template agent includes polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, tetrapropylammonium hydroxide, citric acid, polyvinyl alcohol or polyethylene glycol, The solvent is water, The temperature of the hydrothermal reaction is 100-300°C. The lithiation method is an in-situ electrochemical lithiation method or a chemical lithiation method. The conductive carbon-based material is subjected to modification and acidification treatment before mixing. During the preparation of the multi-dimensional disordered rock salt composite solid electrolyte: The temperature of the in-situ polymerization reaction is 60-90°C.
9. The method for preparing a multi-dimensional disordered rock salt composite material according to claim 8, characterized in that: The conductive carbon-based material is modified and acidified, and the specific process is: mixing the conductive carbon-based material, concentrated nitric acid and concentrated sulfuric acid, stirring, filtering, vacuum drying, and high-speed shear dispersion; The specific process of the in-situ electrochemical lithiation method is: assembling the disordered rock salt composite material into a half-cell, using a lithium-containing electrolyte for charging and discharging, and embedding lithium ions into the disordered rock salt-based composite material under the action of an electric field to obtain a disordered rock salt composite electrode; The half-cell further comprises a negative electrode shell, a spring, a gasket, an electrolyte, a diaphragm, an electrolyte, a lithium sheet, and a positive electrode shell, and the disordered rock salt-based composite material is located between the gasket and the electrolyte; The lithium-containing electrolyte includes lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate; The molar ratio of the disordered rock salt-based composite material to the lithium-containing electrolyte is 1:(1-2); The specific process of the chemical lithiation method is: mixing the disordered rock salt-based composite material with a strong reducing lithium-containing reagent under an inert atmosphere to obtain a disordered rock salt composite electrode; The strong reducing lithium-containing reagents include n-butyl lithium solution, ethyl lithium solution, phenyl lithium solution, and methyl lithium solution; The molar ratio of the disordered rock salt-based composite material to the lithium-containing solution is 1:(3-4).
10. Application of a multidimensional disordered rock salt composite material as described in claim 6 in the field of electrochemical energy storage devices, wherein the electrochemical energy storage devices include lithium metal batteries, lithium ion batteries, supercapacitors, lithium air batteries, and solid electrolytes.