Preparation method of single-crystal high-nickel ternary positive electrode material

The precursor is refined through ball milling-spray drying and combined with lithiated sintering, which solves the microcracks and secondary agglomeration problems of traditional high-nickel ternary positive electrode materials in lithium-ion batteries, and improves the dispersion and electrochemical properties of the materials. , meets the needs of high-energy density lithium-ion batteries.

CN119038629APending Publication Date: 2024-11-29INST OF RESOURCES UTILIZATION & RARE EARTH DEV GUANGDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159534.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional high-nickel ternary cathode materials are prone to problems such as cation mixing, transition metal ion dissolution, irreversible phase change and anisotropic microcracks during charging and discharging of lithium-ion batteries, which affects their commercial application, and the existing preparation methods are difficult to Preparation of single crystal precursors with smaller particle sizes leads to low yield, high cost and poor batch stability.

Method used

The ball mill-spray drying method was used to process the precursor Ni0.83Co0.11Mn0.06 (OH)2 with an average particle size of 3 to 5 μm, and refined to 2.1 to 3.61 μm, and then mixed with zirconium spheres to undergo lithiation sintering. This method improves the dispersion and electrochemical properties of the precursor and avoids secondary agglomeration of single crystal particles.

Benefits of technology

It significantly improves the particle dispersion of single crystal positive electrode materials, improves its comprehensive electrochemical performance, extends the cycle life and improves the electrochemical capacity, avoids secondary agglomeration of single crystal particles with smaller particle sizes, and meets high energy density lithium Requirements for ionic power batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038629A_ABST
    Figure CN119038629A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a single-crystal high-nickel ternary positive electrode material, precursor particles are further refined through a ball milling-spray drying method until the average particle size is 2.1-3.61 [mu] m, the spherical morphology of a precursor is maintained, the dispersity of the precursor is improved, and then the particle dispersity of the single-crystal material prepared through lithiation sintering is obviously improved. Good comprehensive electrochemical performance is shown, and the problem of secondary agglomeration of single crystal particles with relatively small particle sizes is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to a method for preparing a single crystal high-nickel ternary positive electrode material. Background technology:

[0002] The particles of traditional high-nickel ternary positive electrode materials are polycrystalline in morphology, generally micron-sized spherical secondary particles formed by the agglomeration of primary nanoparticles. When lithium-ion batteries are charged and discharged, the polycrystalline high-nickel ternary electrode materials used as positive electrodes have problems such as cation mixing, transition metal ion dissolution, irreversible phase change and anisotropic microcracks, which seriously affect their commercial application. The current modification measures mainly include doping, coating, and the construction of gradient structures or single-crystal morphology particles. Among them, the single-crystal morphology of the ternary positive electrode material is a micron-sized primary particle, which reduces the grain boundaries of the primary particles in the polycrystalline agglomerates, has the advantages of consistent and continuous lattice orientation, orderly crystal plane arrangement, etc., and effectively alleviates the generation of particle microcracks. At the same time, the higher compaction density and its stable material structure can withstand high-voltage (4.5V) electrolytes, thereby obtaining higher electrochemical capacity and longer cycle life, meeting the needs of high-energy-density lithium-ion power batteries.

[0003] The high-temperature solid phase method and the molten salt-assisted method are currently the main methods for synthesizing single-crystal high-nickel ternary positive electrode materials, using a precursor obtained by the coprecipitation method, with an average particle size of about 3 to 15 μm. The particle size and morphology of the precursor have an important influence on the performance of the positive electrode material. In the high-temperature lithiation stage, the precursor with a smaller particle size is conducive to the growth of primary particles, and it is easy to obtain single-crystal particles with good dispersibility; while the precursor with a larger particle size grows from the nanometer size to the micrometer size of the primary particles, and the agglomerates break apart to form single-crystal particles, which requires a higher sintering temperature and a longer sintering time. The average particle size of the current commercial small-particle precursor is 3 to 5 μm. CN113373517A discloses a high-nickel single-crystal small-particle ternary precursor and a continuous preparation method thereof, and obtains a precursor with an average particle size of 3 to 4 μm. Although this method solves the problems of low output, high cost, and poor batch stability in the current intermittent production of small-particle precursors, it is also difficult to prepare precursors with smaller particle sizes. The main reason is that the operating conditions are more stringent and the sphericity and particle size distribution are more difficult to control.

[0004] In order to obtain a precursor with a smaller particle size, CN115863567A discloses a method for preparing a high-rate small-particle single-crystal positive electrode material and its application. The positive electrode material precursor is mixed with a lithium source and sintered at low temperature. The invention uses a jet mill to directly crush the precursor. The average particle size of the material after crushing is 500-1000nm. After sintering at 850-950℃ in the high-temperature section of lithium treatment for 12-24h, a single-crystal positive electrode material with an average particle size of 0.9-1.6μm is prepared. There are fewer single crystal particles in a dispersed state, and the agglomeration phenomenon is still obvious. The grown primary particles have not yet completely separated from the agglomerate. In addition, CN112811475A discloses a single-crystal positive electrode material, a preparation method thereof, and a lithium-ion battery. The method comprises the following steps: airflow crushing of large particles of 8-12μm polycrystalline precursor to obtain a precursor with an average particle size of 0.2-0.6μm, sintering after lithium addition, and obtaining a single-crystal positive electrode material. It can be seen that the refinement of the precursor particles effectively improves the dispersibility of the single crystal particles, but at the same time, the single crystal particles with smaller particle size obtained after lithiation undergo secondary agglomeration. Summary of the invention:

[0005] The purpose of the present invention is to provide a method for preparing a single crystal high-nickel ternary positive electrode material.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a single crystal high nickel ternary positive electrode material comprises the following steps: preparing a precursor Ni having an average particle size of 3 to 5 μm 0.83 Co 0.11 Mn 0.06 (OH)2, mixed with zirconium balls with a particle size of 1-4 mm at a mass ratio of 1:5-10, and deionized water was added at a solid-liquid ratio of 1:4-6, and then ball-milled on a roller mill at a speed of 55-65 rpm for 1-5 hours. After screening, deionized water was added at a solid-liquid ratio of 1:18-20, and the obtained slurry was spray-dried, with the inlet and outlet temperatures of 250°C and 140°C, respectively, to obtain a treated precursor Ni with an average particle size of 2.1-3.61 μm. 0.83 Co 0.11 Mn 0.06 (OH)2, and then lithiation and sintering to prepare single crystal material.

[0008] The lithium sintering is a prior art, comprising the following steps: 0.83 Co 0.11 Mn 0.06(OH)2 and Li2CO3 were fully mixed at a ratio of Li / Me=1.1:1, and sintered in a tubular furnace with an oxygen atmosphere. After ventilating at room temperature for 2 hours, the mixture was heat treated at 500°C at a heating rate of 5°C / min for 4 hours, then heated to 780-900°C and kept for 25 hours. The mixture was naturally cooled to room temperature, and single crystal materials were obtained after grinding and screening.

[0009] The present invention further refines the precursor particles to an average particle size of 2.1 to 3.61 μm by ball milling-spray drying, while maintaining the spherical morphology of the precursor and improving its dispersibility. The single crystal material prepared by lithium sintering has significantly improved particle dispersibility, exhibits good comprehensive electrochemical properties, and avoids the problem of secondary agglomeration of single crystal particles with smaller particle sizes.

[0010] This method can be directly used for commercially available small-particle precursors with an average particle size of 3 to 5 μm, or it can be used in conjunction with the co-precipitation method for batch production of precursors. In the original water washing and drying process of the precursor filter cake, ball milling-spray drying can be used to obtain a 2 to 3 μm precursor.

[0011] The beneficial effects of the present invention are as follows:

[0012] 1) The present invention performs ball milling on the precursor, which, on the one hand, reduces the size of the larger spherical particles of the precursor, and at the same time changes the surface state of the secondary particles and the looseness of the arrangement of the internal primary particles. During the high-temperature lithiation process, the growing primary particles are easy to completely break out of the agglomerate; on the other hand, it can reduce the degree of breakage of the secondary agglomerate particles of the precursor. Even partially detached flaky primary particles can be reaggregated into spherical small particles through spray drying, and fused into a single crystal particle after high-temperature lithiation.

[0013] 2) Spray drying can also prevent the precursor from agglomerating during the drying process after ball milling.

[0014] In summary, the present invention further refines the precursor particles to an average particle size of 2.1 to 3.61 μm by ball milling-spray drying, while maintaining the spherical morphology of the precursor and improving its dispersibility. The single crystal material prepared by lithium sintering has significantly improved particle dispersibility, exhibits good comprehensive electrochemical properties, and avoids the problem of secondary agglomeration of single crystal particles with smaller particle sizes. Description of the drawings:

[0015] Figure 1 This is the SEM image of the single crystal material of Example 1.

[0016] Figure 2 This is the SEM image of the single crystal material of Example 4.

[0017] Figure 3This is the SEM image of the single crystal material of Comparative Example 1.

[0018] Figure 4 This is the SEM image of the single crystal material of Comparative Example 2.

[0019] Figure 5 This is the SEM image of the untreated precursor of Comparative Example 1.

[0020] Figure 6 This is the SEM image of the precursor treated by ball milling and spray drying in Example 1.

[0021] Figure 7 This is the SEM image of the precursor of Comparative Example 2 after ball milling and spray drying. Specific implementation method:

[0022] The following is a further description of the present invention, rather than a limitation of the present invention.

[0023] Assembly and testing of button cells in the following examples: Mix single crystal positive electrode material powder with acetylene black and polyvinylidene fluoride in a ratio of 8:1:1, add N-methylpyrrolidone and stir for 2.5 hours to form a uniform slurry, and evenly coat the slurry on aluminum foil in a coating machine. Put it in a blast drying oven to dry for 2 hours, press it with a roller machine, and then put it in a vacuum drying oven to dry for 12 hours at a temperature of 80°C, and finally cut it into pieces. The pole piece made of positive electrode material is the positive electrode, the lithium sheet is the negative electrode, the porous polypropylene film (Celgard2500) is the diaphragm, and the electrolytes are high-voltage electrolyte 1 (25°C, density: 1.245g / ml; conductivity: 9.84mS / cm) and high-voltage electrolyte 2 (25°C, density: 1.253g / ml; conductivity: 8.65mS / cm). Assemble CR2032 button cells in a glove box filled with argon. Electrochemical tests were performed after the battery was left to stand for 24 hours. Test temperature: room temperature; test voltage range: 2.8~4.5V.

[0024] Example 1

[0025] The precursor Ni with an average particle size of 3.68 μm 0.83 Co 0.11 Mn 0.06 (OH)2 and zirconium balls (Ø4mm) were mixed at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, the mixture was placed on a roller mill and ball milled at 60rpm for 4h. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250℃ and 140℃ respectively. 10g of the precursor Ni with an average particle size of 2.51μm after drying was weighed. 0.83 Co 0.11 Mn 0.06(OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 201.0mAh / g, and the first charge and discharge efficiency was 85.4%; after 100 cycles at 1C, the capacity retention rate was 87.3%; and the 10C discharge capacity reached 145.6mAh / g.

[0026] The single crystal material was used as the positive electrode material and high-voltage electrolyte 2 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 181.2mAh / g, and the first charge and discharge efficiency was 70.0%; after 100 cycles at 1C, the capacity retention rate was 84.4%.

[0027] Example 2

[0028] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 1 hour. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 3.61 μm after drying. 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2.

[0029] The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 188.0mAh / g, and the first charge and discharge efficiency was 77.7%; after 100 cycles at 1C, the capacity retention rate was 82.9%.

[0030] The single crystal material was used as the positive electrode material and high-voltage electrolyte 2 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge capacity was 181.8mAh / g, and the first charge and discharge efficiency was 73.0%; after 100 cycles at 1C, the capacity retention rate was 66.2%

[0031] Example 3

[0032] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 5 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 2.27 μm after drying. 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 202.6mAh / g, and the first charge and discharge efficiency was 83.8%; after 100 cycles at 1C, the capacity retention rate was 87.8%.

[0033] Example 4

[0034] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф1.5 mm) at a mass ratio of 1:10, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 4 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 2.19 μm after drying. 0.83 Co 0.11 Mn 0.06(OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 207.8mAh / g, and the first charge and discharge efficiency was 84.8%; after 100 cycles at 1C, the capacity retention rate was 81.0%.

[0035] Example 5

[0036] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 4 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 2.51 μm after drying. 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 800℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 201.7mAh / g, and the first charge and discharge efficiency was 86.6%; after 100 cycles at 1C, the capacity retention rate was 71.5%.

[0037] Example 6

[0038] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 4 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 2.51 μm after drying. 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 900℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge capacity was 185.7mAh / g, and the first charge and discharge efficiency was 78.6%; after 100 cycles at 1C, the capacity retention rate was 70.2%.

[0039] Example 7

[0040] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 4 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 2.51 μm after drying. 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then the temperature is raised to 780℃ and kept for 30h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge specific capacity was 196.7mAh / g, and the first charge and discharge efficiency was 83.2%; after 100 cycles at 1C, the capacity retention rate was 86.7%.

[0041] Comparative Example 1

[0042] Weigh 10 g of precursor Ni with an average particle size of 3.68 μm 0.83 Co 0.11 Mn 0.06 (OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge capacity was 191.6mAh / g, and the first charge and discharge efficiency was 77.1%; the 1C cycle was 100 weeks, and the capacity retention rate was 81.9%; the 10C discharge capacity was 108.0mAh / g.

[0043] The single crystal material was used as the positive electrode material and high-voltage electrolyte 2 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge capacity was 188.1mAh / g, and the first charge and discharge efficiency was 70.0%; 1C cycle 100 weeks, the capacity retention rate was 72.6%

[0044] Comparative Example 2

[0045] The precursor with an average particle size of 3.68 μm was mixed with zirconium balls (Ф4 mm) at a mass ratio of 1:5, and deionized water was added at a solid-liquid ratio of 1:5. After stirring evenly, they were placed on a roller mill and ball milled at a speed of 60 rpm for 15 hours. After screening, deionized water was added at a solid-liquid ratio of 1:20, and the obtained slurry was spray dried with the inlet and outlet temperatures of 250°C and 140°C, respectively. Weigh 10 g of the precursor Ni with an average particle size of 1.68 μm after drying. 0.83 Co 0.11 Mn 0.06(OH)2, 4.414g Li2CO3, where Li / Me=1.1:1, are fully mixed and the mixed materials are placed in a tubular furnace with an oxygen atmosphere for sintering. After ventilation for 2h at room temperature, heat treatment is performed at 500℃ at a heating rate of 5℃ / min for 4h, and then heated to 850℃ for 25h. Naturally cool to room temperature, grind in a grinding jar, and pass through a 300-mesh sieve to obtain a single crystal material LiNi 0.83 Co 0.11 Mn 0.06 O2. The single crystal material was used as the positive electrode material and high-voltage electrolyte 1 was selected to assemble a button cell to test its electrochemical performance. Among them, the 0.2C first discharge capacity was 194.8mAh / g, and the first charge and discharge efficiency was 77.3%; after 100 cycles at 1C, the capacity retention rate was 81.1%.

[0046] Figure 1 and Figure 2 The single crystal LiNi obtained in Examples 1 and 4 are 0.83 Co 0.11 Mn 0.06 SEM images of O2 materials. Figure 3 ), the single crystal particles obtained by further refinement of the precursor by ball milling-spray drying have significantly improved dispersion and clearer boundaries. The single crystal material particles obtained by ball milling with smaller zirconium balls have better dispersion.

[0047] Comparison between Examples 1 and 3 and Comparative Example 2 shows that, under the same other conditions, in Comparative Example 2, as the ball milling time is extended to 15 h, the precursor particles with smaller particle sizes are fused into larger particles during the high-temperature lithiation process, and some small-size single crystal particles undergo secondary agglomeration. Figure 4 The dispersibility of the particles is not as good as that of Examples 1 and 3.

[0048] from Figure 5 It can be seen that the original morphology of the precursor that has not been ball-milled and spray-dried is a lamellar structure with obvious boundaries. The closely arranged primary particles agglomerate to form secondary particles with a spherical structure. The size of the secondary particles is relatively uniform, but there are still some smaller particles. The precursor can continue to maintain spherical particles after ball-milling-spray drying. Among them, the secondary agglomerate particles of the precursor treated by ball-milling and spray-drying in Example 1 become smaller in size, and the number of spherical small particles increases. The edges and corners of the surface become smooth and flat, and the gap between the primary particles inside becomes larger. Figure 6 However, as the ball milling time increases, the precursor of Comparative Example 2 treated by ball milling and spray drying has more spherical small particles, and the primary particles inside the several larger particles are arranged very loosely and have a rough surface, such as Figure 7As shown. The particle size of the precursor becomes smaller (<2μm), and the single crystal material synthesized by subsequent high-temperature sintering of lithium undergoes secondary agglomeration to form more large particle agglomerates, and the improvement effect of its electrochemical performance is not significant, see Comparative Example 2. Therefore, by comparing Example 1 and Comparative Example 2, it can be seen that the electrode structure using the single crystal high nickel positive electrode material with good dispersibility in Example 1 as the active material is stable, thereby showing the best cycle stability and rate performance, so the ball milling time is no more than 5h.

[0049] Compared with Comparative Example 1, the first charge and discharge efficiency of the synthetic materials of Examples 1-7 is significantly improved, and the cycle stability of the single crystal materials synthesized from the precursors treated by ball milling and spray drying in Examples 1-3 and 7 is also improved.

[0050] In summary, ball milling of the precursor, on the one hand, reduces the size of the larger spherical particles of the precursor, while changing the surface state of the secondary particles and the looseness of the arrangement of the internal primary particles. During the high-temperature lithiation process, the growing primary particles are easy to completely break out of the agglomerates; on the other hand, it can reduce the degree of breakage of the secondary agglomerate particles of the precursor. Even partially detached flaky primary particles can be reaggregated into small spherical particles through spray drying, and fused into a single crystal particle after high-temperature lithiation. In addition, spray drying can also prevent the ball-milled precursor from agglomerating during the drying process, so the initial charge and discharge efficiency of the synthetic material is significantly improved.

Claims

1. A method for preparing a single crystal high nickel ternary positive electrode material, characterized in that: The following steps are involved: The precursor Ni with an average particle size of 3 to 5 μm 0.83 Co 0.11 Mn 0.06 (OH)2, mixed with zirconium balls with a particle size of 1-4 mm at a mass ratio of 1:5-10, and deionized water was added at a solid-liquid ratio of 1:4-6, and then ball-milled on a roller mill at a speed of 55-65 rpm for 1-5 hours. After screening, deionized water was added at a solid-liquid ratio of 1:18-20, and the obtained slurry was spray-dried, with the inlet and outlet temperatures of 250°C and 140°C, respectively, to obtain a treated precursor Ni with an average particle size of 2.1-3.61 μm. 0.83 Co 0.11 Mn 0.06 (OH)2, and then lithiation and sintering to prepare single crystal material.

2. The preparation method according to claim 1, characterized in that: The lithium sintering comprises the following steps: 0.83 Co 0.11 Mn 0.06 (OH)2 and Li2CO3 were fully mixed at a ratio of Li / Me=1.1:1, and sintered in a tubular furnace with an oxygen atmosphere. After ventilating at room temperature for 2 hours, the mixture was heat treated at 500°C at a heating rate of 5°C / min for 4 hours, then heated to 780-900°C and kept for 25 hours. The mixture was naturally cooled to room temperature, and single crystal materials were obtained after grinding and screening.