Silicon carbide modified carbon / carbon composite material and preparation method thereof
By using water glass and water-soluble sugars to prepare silicon carbide-modified carbon/carbon composite materials, the problems of high preparation cost and insufficient performance in the existing technology are solved, and low-cost, high-performance C/C-SiC composite materials are realized.
Patent Information
- Application Number
- CN202411138012.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
AI Technical Summary
Existing methods for preparing C/C-SiC composite materials suffer from high costs, complex equipment, severe fiber damage, and numerous pores and microcracks, which affect the mechanical properties and thermal insulation performance of the materials.
Using water glass and water-soluble sugars as raw materials, silica-modified carbon/carbon composites were prepared through a sol-gel-carbonization process. Subsequently, high-temperature heat treatment was performed to generate silicon carbide-modified carbon/carbon composites, achieving uniform dispersion of silicon carbide in the sugar-carbon matrix while simultaneously carrying out the carbonization process.
It reduces manufacturing costs, improves the mechanical strength and thermal insulation properties of the material, reduces porosity and microcracks, and enhances the overall performance of the material.
Smart Images

Figure HDA0004999957330000011 
Figure HDA0004999957330000021 
Figure HDA0004999957330000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon-carbon composite thermal insulation materials, and specifically relates to a silicon carbide modified carbon / carbon composite material and a preparation method thereof. Background Art
[0002] With the rapid development of aerospace technology, new high-speed aircraft and their power systems have increasingly stringent requirements on the performance of heat protection materials, which usually require them to be able to withstand ultra-high temperatures, resist oxidation and ablation for a long time, and have excellent mechanical properties. Among them, carbon / carbon composites (C / C composites) are considered to be a class of candidate materials for thermal protection systems with great application prospects due to their excellent properties such as light weight, high specific modulus, high specific strength, low thermal expansion coefficient, and wear resistance. However, in ultra-high temperature oxidation environments, the rapid oxidation and ablation of the carbon matrix limit its long-term application in extreme ultra-high temperature environments. Part of the C matrix in the C / C composite is replaced by silicon carbide (SiC) with better antioxidant properties. The resulting C / C-SiC composite material exhibits excellent long-term antioxidant and ablation resistance, which is mainly due to the healing SiO2 produced by SiC oxidation, which can form a protective oxide film to prevent oxygen from quickly dissipating into the material.
[0003] At present, the preparation schemes of C / C-SiC composite materials at home and abroad mainly include chemical vapor infiltration, reactive melt infiltration, slurry impregnation hot pressing, precursor impregnation pyrolysis, chemical liquid vapor deposition and mixed processes. Among them, (1) the chemical vapor infiltration method is prone to "crusting" phenomenon during the preparation process, leaving a large number of residual pores inside the preform, affecting the mechanical properties of the material. In addition, the preparation cost of the chemical vapor infiltration method is high, the equipment is complex, and only one preform can be operated at a time. (2) The reactive melt infiltration method will leave residual Si in the composite material. The residual Si reacts with carbon fiber to damage the fiber, affecting the final mechanical properties of the composite material. (3) The slurry impregnation hot pressing method is not suitable for the preparation of complex structural parts because the powder particles in the slurry are easy to agglomerate and block the pores in the outer layer of the fiber preform. The fiber is easily damaged under high temperature and high pressure sintering conditions. (4) The chemical vapor deposition method can be carried out at a relatively low temperature, which can minimize thermal damage and maintain the integrity of the base material. However, its high equipment cost and high temperature process lead to high preparation cost. In addition, the method is very sensitive to process parameters and the preparation process is complicated. Compared with other preparation schemes, the chemical vapor deposition method has a longer cycle and a relatively low output. (5) The precursor impregnation pyrolysis method is used to prepare carbon / carbon composite materials. The time required to complete the entire process is relatively shorter, which is conducive to cost reduction. At the same time, the processing temperature is relatively low, the damage to carbon fiber is small, the composition of the matrix can be controlled, and it can adapt to a variety of fiber preforms to prepare complex-shaped structural parts. However, the ceramic phase prepared by the precursor impregnation pyrolysis method cannot be synchronized with the carbon matrix, which makes it easy to generate pores or microcracks between the ceramic phase and the carbon matrix. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a silicon carbide modified carbon / carbon composite material and a preparation method thereof. The method has low preparation cost, and the raw materials used are inexpensive water glass and water-soluble sugar substances. The preparation process is simple and quick. At the same time, the impregnation of silicon carbide and the sugar-carbon matrix can be carried out simultaneously, thereby achieving a highly uniform dispersion of silicon carbide and forming a large number of silicon carbide / carbon heterogeneous interfaces inside the carbon / carbon composite material, which is not only beneficial to deflect cracks and improve the overall mechanical strength of the composite material, but also can efficiently scatter phonons, reduce the thermal conductivity of the composite material, and improve its thermal insulation effect.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a silicon carbide modified carbon / carbon composite material, comprising the following steps:
[0007] S1: mixing water glass, water-soluble sugar substances and deionized water to prepare an aqueous solution;
[0008] S2: immersing the carbon fiber preform in an aqueous solution, adjusting the pH value to acidic, and then standing, the aqueous solution is gelled in situ to form a gel, and a gel body wrapping the carbon fiber preform is obtained; taking out the gel body wrapping the carbon fiber preform, removing the surface gel and then carbonizing it, repeating the above S1 and S2 several times, and obtaining a silica-modified carbon / carbon composite material;
[0009] S3: subjecting the silicon dioxide modified carbon / carbon composite material to high temperature heat treatment to obtain a silicon carbide modified carbon / carbon composite material.
[0010] In one embodiment, the water-soluble sugar substance is one or more of sucrose, glucose, maltose and fructose.
[0011] In one embodiment, the usage ratio of water glass, water-soluble sugar substance and deionized water is (5-100) g: (10-200) g: (100-500) mL.
[0012] In one embodiment, an acidic solution is used to adjust the pH value; the pH value is 1 to 6; and the acidic solution is any one of oxalic acid, acetic acid and sulfuric acid.
[0013] In one embodiment, the carbon fiber preform is a carbon fiber felt.
[0014] In one embodiment, the standing time is 10 to 48 hours, and the standing environment is a vacuum environment.
[0015] In one embodiment, the process of removing the surface gel and then performing the carbonization treatment is as follows:
[0016] After removing the surface gel of the gel body wrapping the carbon fiber preform, the temperature is stepwise increased from 80° C. to 1200° C. in an inert atmosphere for carbonization for 1 to 50 hours.
[0017] In one embodiment, the high temperature heat treatment process is as follows:
[0018] The silicon dioxide modified carbon / carbon composite material is placed in a high temperature furnace protected by an inert atmosphere, and the temperature is raised to 1400° C. to 2800° C. for a high temperature heat treatment for 0.5 to 5 hours.
[0019] The present invention also provides a silicon carbide modified carbon / carbon composite material prepared by the above-mentioned preparation method of the silicon carbide modified carbon / carbon composite material, wherein the density of the silicon carbide modified carbon / carbon composite material is 0.3-1.6 g / cm 3 .
[0020] In one embodiment, the crystal phase of silicon carbide in the silicon carbide modified carbon / carbon composite material is α phase, β phase or a mixed phase of α phase and β phase.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a method for preparing a silicon carbide modified carbon / carbon composite material, firstly, a water-soluble sugar substance is used as a carbon source, water glass is used as a silicon source, and water is mixed with water in a certain proportion, then a carbon fiber preform is immersed in the above-mentioned configured aqueous solution, the pH value is adjusted, and a silicon dioxide modified carbon / carbon composite material is obtained through repeated sol-gel-carbonization process, and finally, after high-temperature heat treatment, silicon dioxide and sugar carbon undergo in-situ micro-region carbon thermal reduction reaction through mutual diffusion to generate silicon carbide, and finally a silicon carbide modified carbon / carbon composite material is obtained. The method uses a low-cost high-purity water-soluble sugar substance as a carbon source material, and water glass is used as a silicon source material. The solution viscosity is low, and it can fully penetrate into the interior of the carbon fiber bundle, thereby improving the overall mechanical strength of the composite material. More importantly, the preparation method realizes a highly uniform dispersion of silicon carbide in the sugar carbon matrix, and a large number of heterogeneous interfaces can be formed inside the composite material, thereby improving the mechanical and thermal insulation properties of the material. Moreover, the method can make the impregnation of silicon carbide and the sugar carbon matrix proceed simultaneously, greatly reducing the pores or microcracks generated between the ceramic phase and the sugar carbon matrix. The preparation method has low preparation cost, and the entire preparation process is very simple and quick. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Figures (a) to (e) are optical photographs of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention;
[0024] Figure 2 This is a SEM photo of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention;
[0025] Figure 3 This is a SEM photo of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention;
[0026] Figure 4 The XRD spectrum of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention;
[0027] Figure 5 The compression performance test diagram of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention; Figure (a) is the compression performance of the composite material under different repetition times; Figure (b) is the compression curve diagram of the composite material after 6 repetitions;
[0028] Figure 6 This is an infrared thermal imaging image of a silicon carbide modified carbon / carbon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0030] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0031] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0032] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0033] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0034] The invention provides a silicon carbide modified carbon / carbon composite material and a preparation method thereof.
[0035] On the one hand, a method for preparing a silicon carbide modified carbon / carbon composite material is provided, wherein a high-porosity carbon fiber felt material is used as a carbon fiber preform, which is immersed in an aqueous solution containing water glass and water-soluble sugar substances, and the pH value of the solution is adjusted. A silicon dioxide modified carbon / carbon composite material is obtained through repeated sol-gel-carbonization processes, and finally, after high-temperature heat treatment, an in-situ micro-area carbon thermal reduction reaction occurs through mutual diffusion between silicon dioxide and sugar carbon to generate silicon carbide, thereby finally obtaining a silicon carbide modified carbon / carbon composite material.
[0036] The preparation method comprises the following steps:
[0037] S1: mixing water glass, water-soluble sugar substances and deionized water to prepare an aqueous solution;
[0038] S2: immersing the carbon fiber preform in an aqueous solution, adjusting the pH value to acidic, and then standing, the aqueous solution is gelled in situ to form a gel, and a gel body wrapping the carbon fiber preform is obtained; taking out the gel body wrapping the carbon fiber preform, removing the surface gel and then carbonizing it, repeating the above S1 and S2 several times, and obtaining a silica-modified carbon / carbon composite material;
[0039] S3: subjecting the silicon dioxide modified carbon / carbon composite material to high temperature heat treatment to obtain a silicon carbide modified carbon / carbon composite material.
[0040] The specific steps of the above preparation method are as follows:
[0041] Step 1: Prepare aqueous solution: prepare water glass, water-soluble sugar substance and deionized water into aqueous solution according to a certain proportion;
[0042] Step 2: immersing the carbon fiber preform in the aqueous solution prepared in step 1, adjusting the pH value of the solution with an acidic solution, placing the solution in a vacuum state for 10 to 48 hours, and allowing the aqueous solution to gel in situ to form a gel, thereby obtaining a gel that wraps the carbon fiber preform;
[0043] Step 3: Take out the preform of the gel in the above step 2, remove the surface gel, and carbonize it in an inert atmosphere by stepwise heating from 80°C to 1200°C for 1 to 50 hours to obtain a silica-modified carbon / carbon composite material. Repeat the above steps 1 to 20 times for the composite material to change its density.
[0044] Step 4: Heat the silicon dioxide modified carbon / carbon composite material obtained in step 3 to 1400° C. to 2800° C. in a high-temperature furnace protected by an inert atmosphere for 0.5 to 5 hours to obtain a silicon carbide modified carbon / carbon composite material.
[0045] The specific dosage and process conditions are as follows:
[0046] In step 1, in the aqueous solution, the usage ratio of water glass, water-soluble sugar substance and deionized water is (5-100) g: (10-200) g: (100-500) mL.
[0047] Preferably, the water-soluble sugar substance may be one or a combination of sucrose, glucose, maltose and fructose.
[0048] Preferably, the modulus of the water glass may be 1.5, 2, 2.5, 3, or 3.5.
[0049] In step 2, the gel process specifically includes the following steps: adding an acidic solution to the aqueous solution while stirring to adjust the pH value to 1-6, and then placing it in a vacuum environment for 10-48 hours, and the aqueous solution is in situ gelled and solidified into a transparent gel.
[0050] Preferably, the acidic solution may be any one of oxalic acid, acetic acid and sulfuric acid.
[0051] Preferably, the pH value may be 1, 2, 3, 4, 5, or 6.
[0052] Preferably, the time of being placed in the vacuum environment is, for example, 10 h, 20 h, 30 h, 40 h, or 48 h.
[0053] Preferably, the atmosphere for the heat treatment in step 3 and step 4 may be argon and / or nitrogen.
[0054] On the other hand, a silicon carbide modified carbon / carbon composite material prepared by the above preparation method is provided, and its density is 0.3-1.6 g / cm 3 The crystal phase of silicon carbide in the silicon carbide modified carbon / carbon composite material is α phase, β phase or a mixed phase of α phase and β phase.
[0055] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0056] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0057] Embodiment 1:
[0058] Weigh 100g of glucose and 50g of water glass into a 250mL beaker, add 100mL of deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add acetic acid solution to the solution while stirring to adjust the pH value to 4, and then place it in a vacuum environment for 24h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the surface gel, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 24h to obtain a silicon dioxide modified carbon / carbon composite material. Repeat the above steps 6 times to change the density of the silicon dioxide modified carbon / carbon composite material, and finally obtain a silicon carbide modified carbon / carbon composite material by high-temperature heat treatment at 1400℃ for 2h under nitrogen or / and argon protection.
[0059] Depend on Figure 1 As shown in Figures (a) to (e), the prepared carbon / carbon composite material has good processability and can be processed into different shapes according to needs: square, arched, etc. The test results show that the thermal conductivity of the prepared sample is 0.36W / m·k and the mechanical property is 38.4Mpa.
[0060] Depend on Figure 2 , Figure 3 It can be seen that the microstructure of the prepared carbon / carbon composite material, the fiber surface and the large pores between the fibers are wrapped and filled. In addition, it can be seen that silicon carbide is highly evenly dispersed in the sugar carbon matrix, and a large number of silicon carbide / carbon heterogeneous interfaces are formed inside the carbon / carbon composite material, with a density of 0.6156 g / cm 3 .
[0061] Figure 4 The successful conversion of silicon carbide can be seen through XRD phase analysis. Figure 5 As can be seen from the middle figure (a), the compression performance of the composite material increases significantly with the increase in the number of repetitions. Figure 5 The middle figure (b) is a compression curve of the composite material repeated 6 times, and non-brittle fracture behavior is observed, which is the main feature of damage tolerant C / C composites. Figure 6 The thermal imaging image of the composite material on a heating platform at 300°C for 0 to 90 seconds shows that the composite material has good thermal stability and excellent thermal insulation performance. After heating for 90 seconds, the top of the composite material still maintains room temperature.
[0062] Embodiment 2:
[0063] Weigh 10g of glucose and 5g of water glass into a 250mL beaker, add 100mL of deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add oxalic acid solution to the solution while stirring to adjust the pH value to 4, and then place it in a vacuum environment for 10h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the surface gel, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 30h to obtain a silicon dioxide modified carbon / carbon composite material. The above-mentioned silicon dioxide modified carbon / carbon composite material is subjected to a high-temperature heat treatment at 1400℃ for 2h under the protection of nitrogen or / and argon to obtain a silicon carbide modified carbon / carbon composite material.
[0064] The test results show that the density of the silicon carbide modified carbon / carbon composite material prepared in this embodiment is 0.3g / cm 3 .
[0065] Embodiment 3:
[0066] Weigh 50g of glucose and 10g of water glass into a 250mL beaker, add 100mL of deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add sulfuric acid solution to the solution while stirring to adjust the pH value to 2, and then place it in a vacuum environment for 10h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the surface gel, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 50h to obtain a silicon dioxide modified carbon / carbon composite material. Repeat the above steps 9 times to change the density of the silicon dioxide modified carbon / carbon composite material, and finally obtain a silicon carbide modified carbon / carbon composite material by high-temperature heat treatment at 1400℃ for 2h under nitrogen or / and argon protection.
[0067] The test results show that the density of the silicon carbide modified carbon / carbon composite material prepared in this embodiment is 0.7115 g / cm 3 .
[0068] Embodiment 4:
[0069] Weigh 30g fructose and 10g water glass into a 250mL beaker, add 100mL deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add sulfuric acid solution to the solution while stirring to adjust the pH value to 1, and then place it in a vacuum environment for 24h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the gel on its surface, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 24h to obtain a silicon dioxide modified carbon / carbon composite material. Repeat the above steps 20 times to change the density of the silicon dioxide modified carbon / carbon composite material, and finally obtain a silicon carbide modified carbon / carbon composite material by high-temperature heat treatment at 1550℃ for 2h under nitrogen or / and argon protection.
[0070] The test results show that the density of the silicon carbide modified carbon / carbon composite material prepared in this embodiment is 1.6 g / cm 3 .
[0071] Embodiment 5:
[0072] Weigh 200g sucrose and 100g water glass into a 250mL beaker, add 500mL deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add acetic acid solution to the solution while stirring to adjust the pH value to 6, and then place it in a vacuum environment for 48h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the gel on its surface, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 1h to obtain a silica-modified carbon / carbon composite material. Repeat the above steps 12 times to change the density of the silica-modified carbon / carbon composite material, and finally obtain a silicon carbide-modified carbon / carbon composite material by high-temperature heat treatment at 2800℃ for 0.5h under nitrogen or / and argon protection.
[0073] Embodiment 6:
[0074] Weigh 30g of maltose and 10g of water glass into a 250mL beaker, add 100mL of deionized water, dissolve by magnetic stirring, and then stand to clarify to obtain an aqueous solution. Immerse the carbon fiber felt preform in the prepared aqueous solution and vacuum impregnate for 1h until the carbon fiber felt preform is completely immersed in the aqueous solution. Then, add acetic acid solution to the solution while stirring to adjust the pH value to 4, and then place it in a vacuum environment for 24h. Take out the gel body wrapped around the carbon fiber felt preform, and after removing the gel on its surface, place the gel carbon fiber felt preform in a high-temperature furnace protected by nitrogen or / and argon, and step-wise carbonize from 80℃ to 1200℃ for 24h to obtain a silicon dioxide modified carbon / carbon composite material. Repeat the above steps 12 times to change the density of the silicon dioxide modified carbon / carbon composite material, and finally obtain a silicon carbide modified carbon / carbon composite material by high-temperature heat treatment at 1550℃ for 5h under nitrogen or / and argon protection.
[0075] Among various aerospace materials, C / C composite materials have been playing an important role in the aerospace field due to their excellent properties such as high thermal conductivity, light weight, high specific modulus, high specific strength, low thermal expansion coefficient, and wear resistance. In an inert gas environment, C / C composite materials can withstand a high temperature of 2500°C and maintain a higher mechanical property stability than other materials. Therefore, it is widely used in rocket engine nozzles and missile nose cones. The carbon / carbon composite material of the present invention has excellent thermal insulation performance, light weight, high mechanical properties and other characteristics. Using a high-porosity carbon fiber material as a preform, using water-soluble sugar as a carbon source, and water glass as a silicon source, the impregnation of silicon carbide and sugar-carbon matrix can be carried out simultaneously, which not only makes the gap inside the preform smaller, but also makes the material obtain excellent mechanical strength. Compared with traditional thermal insulation materials, it has huge advantages in mechanical properties such as strength, stiffness, and fatigue resistance, and can be widely used in thermal structural materials of aerospace, military weapons and equipment, etc.
[0076] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a silicon carbide modified carbon / carbon composite material, characterized in that: The following steps are involved: S1: mixing water glass, water-soluble sugar substances and deionized water to prepare an aqueous solution; S2: immersing the carbon fiber preform in an aqueous solution, adjusting the pH value to acidic, and then standing, the aqueous solution is gelled in situ to form a gel, and a gel body wrapping the carbon fiber preform is obtained; taking out the gel body wrapping the carbon fiber preform, removing the surface gel and then carbonizing it, repeating the above S1 and S2 several times, and obtaining a silica-modified carbon / carbon composite material; S3: subjecting the silicon dioxide modified carbon / carbon composite material to high temperature heat treatment to obtain a silicon carbide modified carbon / carbon composite material.
2. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The water-soluble sugar substance is one or more of sucrose, glucose, maltose and fructose.
3. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The usage ratio of the water glass, the water-soluble sugar substance and the deionized water is (5-100) g: (10-200) g: (100-500) mL.
4. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: An acidic solution is used to adjust the pH value; the pH value is 1-6; the acidic solution is any one of oxalic acid, acetic acid and sulfuric acid.
5. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The carbon fiber preform is carbon fiber felt.
6. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The standing time is 10 to 48 hours, and the standing environment is a vacuum environment.
7. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The process of carbonization treatment after removing the surface gel is as follows: After removing the surface gel of the gel body wrapping the carbon fiber preform, the temperature is stepwise increased from 80° C. to 1200° C. in an inert atmosphere for carbonization for 1 to 50 hours.
8. The method for preparing the silicon carbide modified carbon / carbon composite material according to claim 1, characterized in that: The process of high temperature heat treatment is as follows: The silicon dioxide modified carbon / carbon composite material is placed in a high temperature furnace protected by an inert atmosphere, and the temperature is raised to 1400° C. to 2800° C. for a high temperature heat treatment for 0.5 to 5 hours.
9. A silicon carbide modified carbon / carbon composite material obtained according to the method for preparing a silicon carbide modified carbon / carbon composite material according to any one of claims 1 to 8, characterized in that: The density of the silicon carbide modified carbon / carbon composite material is 0.3-1.6 g / cm 3 .
10. The silicon carbide modified carbon / carbon composite material according to claim 9, characterized in that: The crystal phase of silicon carbide in the silicon carbide modified carbon / carbon composite material is α phase, β phase or a mixed phase of α phase and β phase.
Citation Information
Patent Citations
Preparation method of beta-nano-SiC
CN102432013A
Method for preparing anti-oxidation coating of carbon / carbon composite material
CN103030427A
Preparation technology of carbon nanofiber composite silicon dioxide aerogel
CN105418052A
Preparation method of silicon carbide nanometer particles capable of absorbing organic dyes with high efficiency
CN108314050A
Preparation method of ceramic based composite material
CN108409329A