HNIW crystal form regulation and control method based on microfluidic technology
Through microfluidic control technology, the solvent and non-solvent flow rates of HNIW are controlled, and the flexible preparation and precise regulation of HNIW polymorphism is achieved, which solves the problems of uneven particle size and insufficient safety in traditional methods, and improves the safety of the preparation process. Sex and product quality.
Patent Information
- Application Number
- CN202411121086.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for the prior art to achieve flexible preparation and precise regulation of HNIW polymorphic forms, and the HNIW prepared by traditional methods is uneven in particle size, the amount of hazardous goods is large, and the safety is insufficient.
Using a method based on microfluidic control technology, using HNIW as the raw material, ethyl acetate or acetone as the solvent, petroleum ether, n-heptane, deionized water or toluene as the non-solvent, the precision of solvent and non-solvent through the microfluidic chip is carried out. Control to achieve the preparation of α-, β- and ε-type HNIW, including solution preparation, injection of recrystallization module, suspension collection, filtration, washing and freeze-drying steps.
The precise regulation of HNIW crystal form is achieved, which reduces the problem of uneven particle size, improves the safety of the preparation process and the uniformity of the particle size distribution of the product, and reduces the use of dangerous goods.
Smart Images

Figure BDA0004995118100000041 
Figure BDA0004995118100000051 
Figure HDA0004995118110000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of energetic materials and relates to a HNIW crystal form control method based on microfluidic technology. Background Art
[0002] Hexanitrohexaazaisowurtzitane (HNIW) is a typical representative of high energy density materials and can be used as a high-energy component of solid propellants and propellants. HNIW has five crystal forms: α, β, γ, ε and ζ, among which γ-HNIW is a crystal form obtained under high temperature, and ζ is a crystal form obtained under high pressure. In order to obtain HNIW with different crystal forms, crystal form control technology has become the forefront and hot spot of research in the field of explosives. Recrystallization is an effective means of separation and purification. During the recrystallization process of HNIW, its crystal form will also be affected by process parameters. Centuries of research have gradually revealed the essence of crystallization while also raising many new problems. How to obtain crystal products of specified quality in a controllable manner has always been one of the most concerned issues for researchers. At the same time, how to use the same preparation system to achieve flexible preparation of HNIW polymorphs remains to be explored. Summary of the invention
[0003] In view of the deficiencies in the prior art, the object of the present invention is to provide a method for regulating the crystal form of HNIW based on microfluidic technology, and to prepare α-, β- and ε-type HNIW. The method can prepare HNIW of various crystal forms using the same set of equipment, and can achieve precise regulation of the HNIW crystal form according to the product crystal form requirements.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0005] A HNIW crystal form control method based on microfluidic technology, the method uses HNIW as a raw material, ethyl acetate or acetone as a solvent, petroleum ether, n-heptane, deionized water or toluene as a non-solvent, and can prepare α-HNIW, β-HNIW and ε-HNIW by changing different parameters in the same preparation system.
[0006] The present invention also includes the following technical features:
[0007] Specifically, the following steps are included:
[0008] Step 1, completely dissolving HNIW in a solvent to prepare a HNIW solution as a solvent phase;
[0009] Step 2, injecting the solvent phase and the non-solvent into the recrystallization module;
[0010] Step 3, collecting the suspension, filtering, washing, and freeze-drying after the crystals are completely precipitated to obtain HNIW crystals.
[0011] Specifically, the recrystallization module is a microfluidic chip with a specific structure, including but not limited to heart-shaped, S-shaped, and T-shaped microfluidic chips.
[0012] Specifically, the concentration of the solvent phase is 0.1 to 0.3 g / mL.
[0013] Specifically, the flow rate of the solvent phase injected into the recrystallization module is 0.5-1 mL / min.
[0014] Specifically, the flow rate of the non-solvent injected into the recrystallization module is 5 to 20 mL / min.
[0015] Specifically, the injection flow rate ratio of the solvent phase to the non-solvent is 1:10 to 1:20.
[0016] Specifically, in step 3, the detergent used for washing is ethanol or deionized water.
[0017] Specifically, in step 3, the collected suspension is stirred and allowed to stand before filtering.
[0018] Compared with the prior art, the present invention has the following technical effects:
[0019] (1) The present invention can use a set of preparation systems to achieve precise control of HNIW crystal forms and realize flexible preparation of HNIW according to product requirements.
[0020] (2) The present invention takes advantage of the microfluidics in preparing micro-nano energetic materials. The particle size of the prepared HNIW samples is smaller than that of the traditional kettle preparation method and is evenly distributed.
[0021] (3) The preparation method proposed in the present invention can realize continuous product preparation and crystal form control, and the amount of dangerous goods online is small, thereby ensuring the safety of the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the preparation system used in the present invention.
[0023] Figure 2 (a) is the XRD pattern of the HNIW raw material used in the example; (b) is the XRD pattern of α-HNIW prepared in Example 1 of the method of the present invention; (c) is the XRD pattern of β-HNIW prepared in Example 2 of the method of the present invention; (d) is the XRD pattern of ε-HNIW prepared in Example 3 of the method of the present invention.
[0024] Figure 3(a) is a SEM photograph of the HNIW raw material used in the examples; (b) is a SEM photograph of α-HNIW prepared in Example 1 of the method of the present invention; (c) is a SEM photograph of β-HNIW prepared in Example 2 of the method of the present invention; (d) is a SEM photograph of ε-HNIW prepared in Example 3 of the method of the present invention. DETAILED DESCRIPTION
[0025] The present invention provides a HNIW crystal form control method based on microfluidic technology, which uses HNIW as a raw material, ethyl acetate or acetone as a solvent, petroleum ether, n-heptane, deionized water or toluene as a non-solvent, and adjusts the types of solvent and non-solvent used and the post-processing time according to the crystal form of the desired product, so that α-HNIW, β-HNIW and ε-HNIW can be prepared by changing different parameters in the same preparation system. The microfluidic technology involved is a technology that uses microchannels (0.1 μm to 1 mm) to manipulate microfluids. Compared with traditional intermittent reactions, microfluidic chips have higher mass transfer, faster heat transfer rate, less reagent usage and more accurate reaction parameter control.
[0026] The specific steps include:
[0027] Step 1, completely dissolving HNIW in a solvent, stirring with a magnetic force, and preparing an HNIW solution as a solvent phase; the concentration of the solvent phase is 0.1 to 0.3 g / mL.
[0028] Step 2, the driving device such as an injection pump injects the solvent phase and the non-solvent into the recrystallization module microfluidic chip at a certain flow rate; the recrystallization module is a microfluidic chip with a specific structure, including but not limited to heart-shaped, S-shaped, and T-shaped microfluidic chips. Specifically, after the microfluidic chip is washed with the crystallization solvent, the non-solvent is connected to the microfluidic chip, the ratio of the solvent to the non-solvent is adjusted, and the filtrate is collected and processed and collected; the flow rate of the solvent phase injected into the recrystallization module is 0.5 to 1 mL / min; the flow rate of the non-solvent injected into the recrystallization module is 5 to 20 mL / min; the injection flow rate ratio of the solvent phase and the non-solvent is 1:10 to 1:20.
[0029] Step 3, collecting the suspension, filtering, washing, and freeze-drying after the crystals are completely precipitated to obtain HNIW crystals. Specifically, the washing detergent used is ethanol or deionized water; the collected suspension can also be stirred and allowed to stand before filtering.
[0030] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0031] Embodiment 1:
[0032] This embodiment provides a method for controlling the crystal form of HNIW based on microfluidics technology, comprising:
[0033] Solution preparation: Solution A: weigh 3 g HNIW and dissolve it in 10 ml ethyl acetate, stir magnetically for 10 min; Solution B: 100 ml deionized water;
[0034] Sample preparation: Inject solutions A and B into the microfluidic chip through syringe pumps No. 1 and No. 2 at flow rates of 1 ml / min and 10 ml / min, respectively;
[0035] Sample treatment: The collected suspension was filtered, washed with ethanol and freeze-dried for 12 h to obtain α-HNIW; its XRD spectrum is shown in Figure 2 (b), SEM photo Figure 3 (b).
[0036] Embodiment 2:
[0037] This embodiment provides a method for controlling the crystal form of HNIW based on microfluidics technology, comprising:
[0038] Solution preparation: Solution A: weigh 3g HNIW and dissolve it in 10ml ethyl acetate, stir magnetically for 10min; Solution B: 200ml petroleum ether;
[0039] Sample preparation: Inject solutions A and B into the microfluidic chip through syringe pumps No. 1 and No. 2 at flow rates of 1 ml / min and 20 ml / min, respectively;
[0040] Sample treatment: The collected suspension was filtered, washed with ethanol and freeze-dried for 12 h to obtain β-HNIW; its XRD pattern is shown in Figure 2 (c), SEM photo Figure 3 (c).
[0041] Embodiment 3:
[0042] This embodiment provides a method for controlling the crystal form of HNIW based on microfluidics technology, comprising:
[0043] Solution preparation: Solution A: weigh 3g HNIW and dissolve it in 10ml ethyl acetate, stir magnetically for 10min; Solution B: 150ml petroleum ether;
[0044] Sample preparation: Inject solutions A and B into the microfluidic chip through syringe pumps No. 1 and No. 2 at flow rates of 1 ml / min and 15 ml / min, respectively;
[0045] Sample treatment: The collected suspension was magnetically stirred for 30 min and then allowed to stand for 6 h, filtered, washed with ethanol and freeze-dried for 12 h to obtain ε-HNIW; its XRD pattern is shown in Figure 2 (d), SEM photo see Figure 3(d).
[0046] Sample characterization analysis:
[0047] Figure 2 (a), (b), (c), and (d) are the XRD spectra of HINW raw material and α, β, and ε-HNIW prepared by the method of the present invention, respectively. It can be clearly seen that the crystal forms of α, β, and ε-HNIW samples prepared by the method of the present invention are consistent with those of the standard substances. When the non-solvent with a large dipole moment is selected, such as toluene and deionized water, the prepared HNIW are all α-type. When the flow rates of the non-solvent and the solvent are relatively large, it is difficult to reach thermodynamic equilibrium during the recrystallization process. Since the nucleation barrier of the metastable phase β is lower than that of the stable phase ε, a large amount of β-HNIW will be produced first at a high flow ratio, and the increase in supersaturation will increase the number of crystal nuclei and reduce the crystal size. With the increase of processing time, the solution system reaches thermodynamic equilibrium, and ε-HNIW appears. According to Figure 3 The SEM image shows that the raw material particles are uneven in size, irregular in shape, with many sharp edges and corners and many surface defects. In contrast, the particle size of the α, β and ε-HNIW samples prepared by the method of the present invention is significantly reduced, with a narrow particle size distribution and a smooth surface.
[0048] The present invention also provides other embodiments as shown in Table 1, by changing different parameters, the HNIW crystal form is controlled to prepare α-HNIW, β-HNIW or ε-HNIW; wherein the different parameters include: solvent type, non-solvent type, solution concentration, non-solvent to solvent phase flow rate ratio, post-treatment method or duration, detergent type, etc., and other preparation details are the same as the above embodiments.
[0049] Table 1 Effect of changing different parameters on HNIW crystal form
[0050]
[0051]
[0052] The above discussion is based on the optimal embodiment and does not limit the present invention. The various technical features involved can be freely combined under different processes, and will not be described here one by one. Any technician in this field can adjust the process parameters within the scope of the technical solution based on this system, and its essence still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for regulating HNIW crystal form based on microfluidics, characterized in that: The method uses HNIW as a raw material, ethyl acetate or acetone as a solvent, and petroleum ether, n-heptane, deionized water or toluene as a non-solvent. α-HNIW, β-HNIW and ε-HNIW can be prepared by changing different parameters in the same preparation system.
2. The HNIW crystal form control method based on microfluidic technology according to claim 1, characterized in that: The following steps are involved: Step 1, completely dissolving HNIW in a solvent to prepare a HNIW solution as a solvent phase; Step 2, injecting the solvent phase and the non-solvent into the recrystallization module; Step 3, collecting the suspension, filtering, washing, and freeze-drying after the crystals are completely precipitated to obtain HNIW crystals.
3. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: The recrystallization module is a microfluidic chip with a specific structure, including but not limited to heart-shaped, S-shaped, and T-shaped microfluidic chips.
4. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: The concentration of the solvent phase is 0.1-0.3 g / mL.
5. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: The flow rate of the solvent phase injected into the recrystallization module is 0.5-1 mL / min.
6. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: The flow rate of the non-solvent injected into the recrystallization module is 5 to 20 mL / min.
7. The HNIW crystal form control method based on microfluidics technology according to claim 2, characterized in that: The injection flow rate ratio of the solvent phase to the non-solvent is 1:10 to 1:
20.
8. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: In step 3, the detergent used for washing is ethanol or deionized water.
9. The HNIW crystal form control method based on microfluidic technology according to claim 2, characterized in that: In the step 3, the collected suspension is stirred and allowed to stand before filtering.
Citation Information
Patent Citations
Active microfluidic platform-based CL-20 crystal form control method
CN110592677A