MXene-based insulating electromagnetic shielding film and preparation method thereof
By oriented distribution of modified MXene in porous membrane, the contradiction between electromagnetic shielding and insulation of polymer-based electromagnetic shielding materials is solved, and efficient electromagnetic shielding performance and low conductivity are achieved, meeting the high-performance shielding materials of modern electronic equipment. need.
Patent Information
- Application Number
- CN202411256997.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
The existing polymer-based electromagnetic shielding materials are difficult to maintain electrical insulation while improving electromagnetic shielding performance, resulting in a contradiction between electromagnetic interference shielding and insulation, which cannot meet the needs of modern electronic equipment for high-performance shielding materials.
Using MXene-based insulated electromagnetic shielding film, the MXene-based insulated electromagnetic shielding film is stripped off and modified with polyethyleneimine. Combined with the palliative characteristics of Plannik F127, the modified MXene is directionally distributed in the porous membrane to achieve high conductivity and overall insulation. balance.
Achieving electromagnetic shielding performance of more than 30dB in the frequency band of 8.2~12.4GHz, and maintaining conductivity below 2.0×10-7S/m in the frequency range of 10~106Hz, meeting the demand for high-performance shielding materials of modern electronic equipment. The preparation method is simple, environmentally friendly and low cost.
Smart Images

Figure CN119039758A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electromagnetic interference shielding composite materials, and specifically relates to a MXene-based insulating electromagnetic shielding film and a preparation method thereof. Background Art
[0002] Electromagnetic interference generated during the operation of electronic devices can cause electronic equipment failures and endanger the health of humans and other organisms. With the increasing application of highly integrated electronic devices in daily life, the demand for materials with high electromagnetic interference shielding capabilities has increased dramatically to protect the normal operation of electronic devices and human health. Polymer-based electromagnetic shielding materials are conductive polymer composites prepared with polymers as the matrix and filled with conductive fillers. They have attracted widespread attention due to their light weight, easy processing, low density and strong flexibility. At the same time, electromagnetic shielding materials should also have electrical insulation to ensure the safety of equipment operation.
[0003] At present, the development of polymer-based electromagnetic shielding materials with electrical insulation properties is still quite challenging. First, materials with high electrical conductivity can provide better electromagnetic shielding effects because they can reduce electromagnetic interference by reflecting and absorbing electromagnetic waves. However, the conductive fillers in excellent electromagnetic interference shielding materials will inevitably destroy the electrical insulation of the polymer, making it difficult to achieve good electrical insulation performance. For example, some metals and metal-based composite materials have shown excellent performance in the field of electromagnetic shielding. However, high conductivity may cause unexpected electrical short circuits or interference in electronic devices, and additional insulating layers are required in some applications to prevent electrical short circuits or interference. Secondly, enhancing insulation performance requires reducing free electrons, or adding insulating materials to electromagnetic shielding materials will hinder the migration of free electrons, reduce the system's ability to attenuate electromagnetic waves, and is not conducive to improving electromagnetic shielding performance. Such materials include some wood-based electromagnetic shielding materials and polymer materials with good insulation properties, which have significant advantages in maintaining electrical safety. However, it is the low conductivity characteristics of these materials that limit their performance in electromagnetic shielding effectiveness. Therefore, how to solve the contradiction between electromagnetic shielding and electrical insulation in existing materials is a problem that technicians in this field need to solve urgently. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a MXene-based insulating electromagnetic shielding film and a preparation method thereof, in view of the fact that existing excellent electromagnetic shielding films often rely on the addition of a large amount of conductive fillers, resulting in increased material conductivity and possibly failing to meet the insulation performance requirements of precision electronic devices. The present invention balances electromagnetic shielding effectiveness and electrical insulation performance through material innovation, structural design, interface optimization and other means to meet the demand for high-performance shielding materials in modern electronic devices.
[0005] Specifically, a single layer of MXene is first peeled off and modified with polyethyleneimine to obtain a modified MXene. Then, the amphiphilic properties of Pluronic F127 are utilized and used as an anchoring agent to prepare a porous membrane by a phase inversion method while the modified MXene is directional distributed on the pore wall of the porous membrane. The interaction between the hydrophobic segments of Pluronic F127 and the polymer matrix anchors it on the pore surface of the polymer porous membrane, while the interaction between the hydrophilic segments of Pluronic F127 and the modified MXene causes the modified MXene to be distributed on the pore wall of the porous membrane, achieving the effect of high conductivity and overall insulation of the modified MXene in a single honeycomb pore. The prepared MXene-based insulating electromagnetic shielding film has an electromagnetic shielding effectiveness of more than 30dB in the 8.2-12.4GHz frequency band and 10-10 6 The conductivity in the Hz frequency range is maintained at 2.0×10 -7 S / m or less.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The first technical purpose of the present invention is to provide a MXene-based insulating electromagnetic shielding film, which is composed of 60-95wt% of a honeycomb porous polymer, 5-40wt% of a modified MXene and 2-10wt% of Pluronic F127, wherein the modified MXene is distributed on the pore walls of the honeycomb porous polymer.
[0008] It should be noted that the electromagnetic shielding effectiveness of the MXene-based insulating electromagnetic shielding film is above 30 dB in the frequency range of 8.2 to 12.4 GHz, and the electromagnetic shielding effectiveness of the MXene-based insulating electromagnetic shielding film is above 30 dB in the frequency range of 10 to 10 6 The conductivity in the Hz frequency range is maintained at 2.0×10 -7 S / m or less.
[0009] Furthermore, the polymer matrix of the honeycomb porous polymer of the above-mentioned MXene-based insulating electromagnetic shielding film is one of polyarylethernitrile, polyaryletherketone, polyarylethersulfone, polyimide, polyetherimide, polyvinylidene fluoride, polystyrene, polymethyl methacrylate, polyethylene, and polypropylene.
[0010] Furthermore, the preparation method of the modified MXene specifically comprises the following steps:
[0011] M1. Mix lithium fluoride and 37% concentrated hydrochloric acid in a PTFE container and stir continuously for 10 to 30 minutes to obtain a uniform mixture, then add titanium aluminum carbide, stir and etch at 30 to 60° C. for 24 to 48 hours, wherein the mass ratio of titanium aluminum carbide to lithium fluoride is 0.5:1 to 1:1, and the mass ratio of 37% concentrated hydrochloric acid to lithium fluoride is 10:1 to 100:1;
[0012] M2, centrifuge the product of M1 at 1000-5000 rpm for 5-30 min to remove the supernatant, and repeatedly wash the lower solid with deionized water and centrifuge in a centrifuge tube until the pH value reaches 7.0;
[0013] M3, pour the above M2 product into 10-100 times the mass of deionized water, ultrasonicate it at 50-500W for 1-2h, further centrifuge it at 1000-5000rpm for 30-60min to remove the large pieces of unpeeled MAX product, and then filter the supernatant to obtain MXene;
[0014] M4. Add the MXene obtained in the above M3 into deionized water, and ultrasonicate it in an ice water bath at 10-100W ultrasound for 1-2 hours to obtain a dispersion with a mass concentration of MXene of 5-30wt%, and then add polyethyleneimine to the above dispersion, stir at a speed of 100-500rpm for 3-8h, and then centrifuge at 3000-10000rpm for 30-60min to obtain a solid product, and finally vacuum dry it at room temperature for 24-48h to obtain a modified MXene, wherein the mass ratio of polyethyleneimine to MXene is 0.5:1-5:1.
[0015] A further beneficial effect of the above method is that the MXene after etching and stripping is a nanomaterial with excellent conductive properties; and the surface of MXene is electronegative, and the electropositive polyethyleneimine can be coated on the surface of MXene through electrostatic action to achieve MXene modification.
[0016] The second technical purpose of the present invention is to provide a method for preparing the above-mentioned MXene-based insulating electromagnetic shielding film, the steps of which are as follows:
[0017] S1. Add modified MXene and polyvinyl pyrrolidone to N-methyl pyrrolidone A, and stir at a speed of 100 to 500 rpm for 1 to 3 hours to obtain a mixture, wherein the mass ratio of modified MXene to polyvinyl pyrrolidone is 0.5:1 to 7.5:1, and the mass ratio of N-methyl pyrrolidone A to modified MXene is 20:1 to 100:1;
[0018] S2, adding the polymer matrix and Pluronic F127 to N-methylpyrrolidone B, stirring at a speed of 100-500 rpm for 1-3 hours to obtain a uniform solution, wherein the mass ratio of the polymer matrix to the modified MXene is 4:1-15:1, the mass ratio of Pluronic F127 to the modified MXene is 0.1:1-2:1, and the mass of N-methylpyrrolidone B is 1-3 times that of N-methylpyrrolidone A;
[0019] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 100 to 500 rpm for 10 to 30 min, and then pouring it onto a glass substrate and scraping it into a liquid film of 100 to 2000 μm using a film scraper;
[0020] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 to 4 hours to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 to 48 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 to 48 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0021] The further beneficial effect of adopting the above method is that the polyethyleneimine and polyvinyl pyrrolidone on the surface of the modified MXene in step S1 are both hydrophilic polymers, and the interaction between the two is strong. Mixing in advance helps to drive the modified MXene to move to the polymer-poor phase during the phase inversion process; the polymer matrix and Pluronic F127 in step S2 are both hydrophobic polymers, and the interaction between the two is strong. Mixing in advance helps to anchor Pluronic F127 on the pore surface of the polymer porous membrane during the phase inversion process, and the interaction between the hydrophilic segments of Pluronic F127 and polyethyleneimine and polyvinyl pyrrolidone can make the modified MXene distributed on the pore wall of the porous membrane, so as to achieve the effect of high conductivity and overall insulation of the modified MXene in a single honeycomb pore.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The present invention aims at the problem that electromagnetic shielding and insulation performance are difficult to be compatible. On the one hand, the electromagnetic shielding material with a porous structure is designed. The pore wall provides multiple interfaces, allowing the reflection and absorption of electromagnetic radiation in the material, and using a small amount of conductive filler to achieve higher electromagnetic shielding performance. On the other hand, the modified MXene is distributed in a direction on the pore wall of the porous film, achieving the effect of high conductivity in a single honeycomb pore and overall insulation of the film.
[0024] 2) The electromagnetic shielding effectiveness of the insulating electromagnetic shielding film of the present invention is above 30dB in the frequency band of 8.2 to 12.4GHz and above 10 to 10 6 The conductivity in the Hz frequency range is maintained at 2.0×10 -7 S / m or less.
[0025] 3) The preparation method of the MXene-based insulating electromagnetic shielding film of the present invention is simple to operate, environmentally friendly, has low equipment requirements and cost, and is suitable for practical application and large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0027] Figure 1 This is a SEM image of the MXene-based insulating electromagnetic shielding film prepared in Example 4 of the present invention;
[0028] Figure 2 The electromagnetic shielding performance of the MXene-based insulating electromagnetic shielding film prepared in Example 4 of the present invention;
[0029] Figure 3 The electrical conductivity of the MXene-based insulating electromagnetic shielding film prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0032] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0033] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0034] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0035] The invention discloses a MXene-based insulating electromagnetic shielding film and a preparation method thereof.
[0036] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0037] Example 1
[0038] Preparation of modified MXene:
[0039] M1. Mix 1.6 g of lithium fluoride and 24 g of 37% concentrated hydrochloric acid in a PTFE container and stir continuously for 10 min to obtain a uniform mixture, then add 1 g of titanium aluminum carbide and stir and etch at 40° C. for 48 h;
[0040] M2, centrifuge the product of M1 at 3500 rpm for 5 min to remove the supernatant, and repeatedly wash the lower solid with deionized water and centrifuge in a centrifuge tube until the pH value reaches 7.0;
[0041] M3, 0.5 g of the above M2 product was poured into 20 g of deionized water, ultrasonicated at 100 W for 2 h, and further centrifuged at 5000 rpm for 30 min to remove large pieces of unpeeled MAX product, and the supernatant was filtered to obtain MXene;
[0042] M4. Add 0.3 g of MXene obtained in the above M3 to 2.7 g of deionized water, and ultrasonicate in an ice-water bath at 100 W for 1 hour to obtain a dispersion with a mass concentration of 10 wt% of MXene. Then add 0.3 g of polyethyleneimine to the above dispersion, stir at 450 rpm for 3 hours, and then centrifuge at 8000 rpm for 30 minutes to obtain a solid product. Finally, vacuum dry at room temperature for 24 hours to obtain the modified MXene.
[0043] Preparation of MXene-based insulating electromagnetic shielding films:
[0044] S1, adding 0.09 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0045] S2, adding 0.87 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0046] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0047] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0048] The prepared MXene-based insulating electromagnetic shielding film has an electromagnetic shielding of 31.6 dB at 8.2 GHz and a 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0049] Example 2
[0050] Preparation of modified MXene: consistent with Example 1.
[0051] Preparation of MXene-based insulating electromagnetic shielding films:
[0052] S1, adding 0.09 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0053] S2, adding 0.87 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0054] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then pouring the mixture onto a glass substrate and scraping it into a 1000 μm liquid film with a film scraper;
[0055] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0056] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 46.4 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.9×10 -7 S / m.
[0057] Example 3
[0058] Preparation of modified MXene: consistent with Example 1.
[0059] Preparation of MXene-based insulating electromagnetic shielding films:
[0060] S1, adding 0.09 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0061] S2, adding 0.87 g of polyaryletherketone and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0062] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0063] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0064] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 31.4 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0065] Example 4
[0066] Preparation of modified MXene: consistent with Example 1.
[0067] Preparation of MXene-based insulating electromagnetic shielding films:
[0068] S1, adding 0.12 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0069] S2, adding 0.84 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0070] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0071] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0072] The scanning electron microscope image of the prepared insulating electromagnetic shielding film is shown in the attached figure. Figure 1 As shown in the figure, the electromagnetic shielding at 8.2GHz is 32.8dB. Figure 2 As shown, in 10 6 The conductivity value at Hz is 1.8×10 -7 S / m, as attached Figure 3 shown.
[0073] Example 5
[0074] Preparation of modified MXene: consistent with Example 1.
[0075] Preparation of MXene-based insulating electromagnetic shielding films:
[0076] S1, adding 0.15 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0077] S2, adding 0.81 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0078] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0079] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0080] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 41.2 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 2.0×10-7 S / m.
[0081] Example 6
[0082] Preparation of modified MXene: consistent with Example 1.
[0083] Preparation of MXene-based insulating electromagnetic shielding films:
[0084] S1, adding 0.09 g of modified MXene and 0.04 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0085] S2, adding 0.85 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0086] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0087] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0088] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 31.3 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0089] Example 7
[0090] Preparation of modified MXene: consistent with Example 1.
[0091] S1, adding 0.09 g of modified MXene and 0.06 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0092] S2, adding 0.83 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0093] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0094] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0095] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 30.9 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0096] Example 8
[0097] Preparation of modified MXene: consistent with Example 1.
[0098] Preparation of MXene-based insulating electromagnetic shielding films:
[0099] S1, adding 0.09 g of modified MXene and 0.08 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0100] S2, adding 0.81 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0101] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0102] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0103] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 30.4 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0104] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0105] Comparative Example 1
[0106] Preparation of MXene:
[0107] M1. Mix 1.6 g of lithium fluoride and 24 g of 37% concentrated hydrochloric acid in a PTFE container and stir continuously for 10 min to obtain a uniform mixture, then add 1 g of titanium aluminum carbide and stir and etch at 40° C. for 48 h;
[0108] M2, centrifuge the product of M1 at 3500 rpm for 5 min to remove the supernatant, and repeatedly wash the lower solid with deionized water and centrifuge in a centrifuge tube until the pH value reaches 7.0;
[0109] M3, 0.5 g of the above M2 product was poured into 20 g of deionized water, ultrasonicated at 100 W for 2 h, and further centrifuged at 5000 rpm for 30 min to remove large pieces of unpeeled MAX product, and the supernatant was filtered to obtain MXene;
[0110] Preparation of MXene-based electromagnetic shielding films:
[0111] S1. Add 0.09 g MXene and 0.02 g polyvinyl pyrrolidone to 3 g N-methylpyrrolidone A, and stir the mixture at 500 rpm for 1 h.
[0112] S2, adding 0.87 g of poly(arylene ether nitrile) and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0113] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0114] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0115] The prepared insulating electromagnetic shielding film has an electromagnetic shielding value of 36.5 dB at 8.2 GHz and a conductivity value of 20 S / m.
[0116] Comparative Example 2
[0117] Preparation of modified MXene: consistent with Example 1.
[0118] Preparation of MXene-based insulating electromagnetic shielding films:
[0119] S1, adding 0.09 g of modified MXene and 0.02 g of polyvinyl pyrrolidone to 3 g of N-methylpyrrolidone A, and stirring the mixture at a speed of 500 rpm for 1 h;
[0120] S2, adding 0.89 g of poly(arylene ether nitrile) to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0121] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0122] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0123] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 18.1 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0124] Comparative Example 3
[0125] Preparation of modified MXene: consistent with Example 1.
[0126] Preparation of MXene-based insulating electromagnetic shielding films:
[0127] S1, adding 0.09 g of modified MXene to 3 g of N-methylpyrrolidone A, and stirring the mixture at 500 rpm for 1 h;
[0128] S2, adding 0.89 g of polyarylethernitrile and 0.02 g of Pluronic F127 to 9 g of N-methylpyrrolidone B, and stirring at 500 rpm for 1 h to obtain a uniform solution;
[0129] S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, stirring at a speed of 500 rpm for 30 min, and then casting the mixture onto a glass substrate and scraping it into a 500 μm liquid film with a film scraper;
[0130] S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol for 1 hour to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol for 12 hours to wash away the polyvinyl pyrrolidone therein, and dried at room temperature for 24 hours to obtain a MXene-based insulating electromagnetic shielding film.
[0131] The electromagnetic shielding performance of the prepared insulating electromagnetic shielding film is 24.3 dB at 8.2 GHz and 10 6 The conductivity value at Hz is 1.5×10 -7 S / m.
[0132] Performance Testing
[0133] The MXene-based insulating electromagnetic shielding films prepared in Examples 1-8 and the porous films prepared in Comparative Examples 1-3 were respectively taken, and the volume resistivity of the samples was tested by a four-point probe resistivity meter using a standard four-probe method.
[0134] The electromagnetic shielding performance of the sample was tested using a waveguide method using a vector network analyzer, where the sample size was a 22.9 mm × 10.2 mm × 2 mm disc, and the test frequency was 8.2-12.4 GHz.
[0135] The results are shown in Table 1.
[0136] Table 1 Electromagnetic shielding and conductivity of films of Examples 1-8 and Comparative Examples 1-3
[0137]
[0138]
[0139] It can be seen from Table 1 that the electromagnetic shielding films prepared in Examples 1-8 have an electromagnetic shielding performance higher than 30 dB and a -7 The conductivity of S / m shows the insulating electromagnetic shielding performance; in Comparative Example 1, due to the addition of unmodified MXene, although it has excellent electromagnetic shielding performance, the conductivity is significantly increased, indicating that modified MXene plays an important role in improving insulation; Comparative Examples 2 and 3 are respectively not added with Pluronic F127 and polyvinyl pyrrolidone, and the prepared electromagnetic shielding films are both insulating, but the electromagnetic shielding of the electromagnetic shielding films is below 30 dB in the frequency band of 8.2 to 12.4 GHz, mainly because the modified MXene fails to be directionally dispersed in the pore wall of the porous membrane, so the addition of Pluronic F127 and polyvinyl pyrrolidone is necessary.
[0140] The above experiments show that the present invention uses the phase inversion method to obtain a porous membrane with a honeycomb pore structure, and can directional distribute the modified MXene on the honeycomb pore wall to achieve the effect of high conductivity and overall insulation in a single honeycomb pore. The insulating electromagnetic shielding film maintains an electromagnetic shielding of more than 30dB in the 8.2-12.4GHz frequency band and 6 The conductivity in the Hz frequency range is lower than 2.0×10 -7 S / m; and the preparation method of the insulating electromagnetic shielding film of the present invention is simple to operate, environmentally friendly, has low equipment requirements and cost, and is suitable for practical application and large-scale production.
[0141] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A MXene-based insulating electromagnetic shielding film, It is characterized in that The MXene-based insulating electromagnetic shielding film is composed of 60-95wt% of a honeycomb porous polymer, 5-40wt% of a modified MXene and 2-10wt% of Pluronic F127, wherein the modified MXene is distributed on the pore walls of the honeycomb porous polymer; The electromagnetic shielding effectiveness of the MXene-based insulating electromagnetic shielding film is above 30 dB in the frequency range of 8.2 to 12.4 GHz; The MXene-based insulating electromagnetic shielding film has a 6 The conductivity in the Hz frequency range is maintained at 2.0×10 - 7 S / m or less.
2. The MXene-based insulating electromagnetic shielding film according to claim 1, It is characterized in that The polymer matrix of the honeycomb porous polymer is one of polyarylethernitrile, polyaryletherketone, polyarylethersulfone, polyimide, polyetherimide, polyvinylidene fluoride, polystyrene, polymethyl methacrylate, polyethylene and polypropylene.
3. The MXene-based insulating electromagnetic shielding film according to claim 1, It is characterized in that The steps of the preparation method of the modified MXene are as follows: M1. Mix lithium fluoride and 37% concentrated hydrochloric acid in a PTFE container and stir to obtain a uniform mixture, then add titanium carbide aluminum for etching reaction; M2, centrifuge the product of M1 to remove the supernatant, and repeat the deionized water washing and centrifugation until the pH is neutral; M3, pour the above M2 product into deionized water, remove the large pieces of unpeeled MAX product after ultrasonication and centrifugation, and then filter the supernatant to obtain MXene; M4. Add the MXene obtained in the above M3 into deionized water, and ultrasonicate in an ice-water bath to obtain a dispersion containing MXene. Then add polyethyleneimine to the above dispersion, stir, and centrifuge to obtain a solid product. Finally, vacuum dry at room temperature to obtain the modified MXene.
4. The MXene-based insulating electromagnetic shielding film according to claim 3, It is characterized in that In M1, the mass ratio of titanium aluminum carbide to lithium fluoride is 0.5:1-1:1, and the mass ratio of 37% concentrated hydrochloric acid to lithium fluoride is 10:1-100:1; the etching reaction temperature is 30-60°C, and the reaction time is 24-48h.
5. The MXene-based insulating electromagnetic shielding film according to claim 3, It is characterized in that In M3, the amount of deionized water used is 10 to 100 times that of the M2 product, the ultrasonic power is 50 to 500 W, and the ultrasonic time is 1 to 2 h.
6. The MXene-based insulating electromagnetic shielding film according to claim 3, It is characterized in that In M4, the ultrasonic power is 10-100 W, the ultrasonic time is 1-2 h; the mass concentration of the dispersion containing MXene is 5-30 wt%; the mass ratio of polyethyleneimine to MXene is 0.5:1-5:
1.
7. A method for preparing the MXene-based insulating electromagnetic shielding film as claimed in claim 1, It is characterized in that The preparation method comprises the following steps: S1. Adding modified MXene and polyvinyl pyrrolidone to N-methylpyrrolidone A, and stirring to obtain a mixture; S2, adding the polymer matrix and Pluronic F127 into N-methylpyrrolidone B, and stirring to obtain a uniform solution; S3, mixing the mixture obtained in S1 and the uniform solution obtained in S2, then casting the mixture onto a glass substrate, and scraping it into a liquid film of 100 to 2000 μm using a film scraper; S4. Immerse the liquid film of S3 together with the glass substrate in anhydrous ethanol to solidify the liquid film and separate it from the glass substrate. The product is further immersed in anhydrous ethanol to wash away the polyvinyl pyrrolidone therein, and dried at room temperature to obtain a MXene-based insulating electromagnetic shielding film.
8. The method for preparing the MXene-based insulating electromagnetic shielding film according to claim 7, It is characterized in that In S1, the mass ratio of the modified MXene to polyvinyl pyrrolidone is 0.5:1 to 7.5:1, and the mass ratio of N-methylpyrrolidone A to the modified MXene is 20:1 to 100:
1.
9. The method for preparing the MXene-based insulating electromagnetic shielding film according to claim 7, It is characterized in that In S2, the mass ratio of the polymer matrix to the modified MXene is 4:1-15:1, the mass ratio of Pluronic F127 to the modified MXene is 0.1:1-2:1, and the mass of N-methylpyrrolidone B is 1-3 times that of N-methylpyrrolidone A.