Feeding method for absorbing iron-rich red mud in molten iron pretreatment process
Patent Information
- Application Number
- CN202411211519.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the existing molten iron pretreatment process, the mechanical stirring method has problems such as large consumption of pretreatment agent and large temperature drop of molten iron, making it difficult to effectively utilize iron resources in iron-rich red mud and LT dry dust removal ash.
Mix iron-rich red mud, LT dry dust removal ash and limestone in a specific proportion, spray it into the iron with nitrogen gas stream, and stir it twice through the stirring head to form compound calcium ferrite, which promotes its uniform dispersion in the iron, and achieves Recycling and utilization of resources and reducing the consumption of pretreatment agents.
The iron resources and valuable minerals in iron-rich red mud and LT dry dust removal ash are recovered, which reduces the consumption of pretreatment agents, reduces the temperature drop of molten iron, and improves the slag removal effect and blowing efficiency.
Smart Images

Figure CN119040544A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of iron and steel smelting resources, and in particular to a feeding method for absorbing iron-rich red mud in a molten iron pretreatment process. Background Art
[0002] Converter dust ash generally refers to the fine dust obtained after dry dust removal from the flue gas generated during the converter blowing process. Converter dust ash contains a large amount of basic oxides such as CaO, and has the characteristics of high iron content, fine particle size, and large specific surface area. Among them, the iron element mainly exists in the form of Fe3O4 and Fe2O3. Converter dust ash is a high-quality iron-containing resource, but due to the high content of basic oxides and fine particle size, it is not only corrosive, but also prone to spontaneous combustion.
[0003] Red mud is a byproduct of the production of alumina from bauxite. It is reddish brown because it contains a large amount of hematite. Red mud has a large output and high alkalinity. If it is discharged into the ocean and / or stored on land using traditional treatment methods, it will seriously pollute seawater, air and soil, not only occupying a large space, but also posing serious ecological and environmental safety risks. It is also a waste of resources.
[0004] Hot metal pretreatment refers to a process of removing impurity elements or recovering valuable elements before adding hot metal to the steelmaking furnace. Hot metal pretreatment processes can be divided into two categories: ordinary hot metal pretreatment and special hot metal pretreatment. Ordinary hot metal pretreatment includes hot metal desulfurization, hot metal desiliconization and hot metal dephosphorization. Special hot metal pretreatment is generally a treatment process for purifying and refining special elements contained in hot metal or comprehensive resource utilization, such as hot metal vanadium extraction, niobium extraction, tungsten extraction, chromium removal and other pretreatment processes.
[0005] Hot metal pretreatment is an important process before steelmaking, which aims to improve the quality of hot metal and increase smelting efficiency. The main methods of hot metal pretreatment include the iron ditch bulk method, the hot metal ladle spraying method and the mechanical stirring method. The iron ditch bulk method is to scatter the pretreatment agent on the hot metal in the iron ditch when the blast furnace is tapped, and use the impact turbulent motion of the hot metal flow to stir and mix the hot metal and the pretreatment agent. This method is simple and easy, but the removal efficiency of harmful elements fluctuates greatly and seriously pollutes the environment. The hot metal ladle spraying method is to spray the pretreatment agent into the hot metal in the hot metal ladle with a spray gun to make it fully react with the hot metal. This method can make the pretreatment agent contact well with the hot metal, and the removal efficiency of harmful elements is high, but the temperature drop of the hot metal is large and the operating cost is high. Mechanical stirring method (KR method) is a method of stirring to make the pretreatment agent placed on the surface of molten iron effectively contact with the molten iron. The KR method can be used for deep purification of molten iron, which can effectively improve the removal efficiency of harmful elements and has low operating costs. It is widely used at home and abroad, but there are also problems such as large temperature drop of molten iron and large consumption of pretreatment agent. Summary of the invention
[0006] In view of the problem of large consumption of pretreatment agent in the prior art of pretreatment of molten iron by mechanical stirring, the present invention provides a feeding method for absorbing iron-rich red mud in the molten iron pretreatment process, wherein the molten iron is pretreated by using iron-rich red mud, LT dry dust removal ash and limestone, thereby realizing the recovery and utilization of iron resources and valuable minerals in solid wastes such as iron-rich red mud and LT dry dust removal ash, and reducing the consumption of pretreatment agent.
[0007] The technical solution of the present invention is as follows: A feeding method for absorbing iron-rich red mud in a molten iron pretreatment process comprises the following steps: Step 1: using a feeding device to evenly mix the iron-rich red mud, LT dry dust removal ash and limestone to obtain a mixed material; Step 2: Spray the mixed material into the molten iron using a nitrogen gas flow, lower the stirring head to stir the molten iron for the first time, and after the first stirring is completed, lift the stirring head to the waiting position; Step 3: lower the stirring head to stir the molten iron for the second time. After the second stirring is completed, lift the stirring head to the waiting position; Step 4: Transport the molten iron to the converter, add scrap steel and then blow it.
[0008] Furthermore, in the mixed material, the mass ratio of iron-rich red mud, LT dry dust removal ash and limestone is 4-5:2-2.5:1.
[0009] Furthermore, in the mixed material, the total content of CaO is 15wt%-25wt%; the total content of SiO2 is 2wt%-2.5wt%.
[0010] Furthermore, in step 2, the amount of mixed material added per ton of steel is calculated according to the following formula: , G is the amount of steel added per ton of mixed material, in kg / t; G0 is the average value of the amount of mixed material added per ton of steel in the current year, in kg / t; T is the temperature of the molten iron in this batch, in °C; T 平均 The average temperature of molten iron in each furnace in this shift, in °C; (Si+P) is the sum of the contents of Si and P in the molten iron of this batch, in wt%; (Si+P) 平均 It is the average value of the sum of the contents of Si and P in each heat of molten steel in this shift, in wt%; T 经验 is the average value of molten iron temperature in the history of this year, in °C. is the correction coefficient of the molten iron temperature of this batch; t 预熔 The pre-melting time of limestone is in minutes. The pre-melting time of limestone is the predicted time from the time when the mixed material is sprayed into the molten iron to the start of blowing. 预熔经验 is the average value of limestone pre-melting time in the current year, in min. is the correction factor for limestone premelting time; t 分解 The theoretical calculation time for limestone to decompose into CaO and CO2, in min, t 分解经验 The time it takes for limestone to decompose into CaO and CO2 is the average value of the historical furnaces this year, in minutes. Correction factor for the theoretical calculation time of limestone decomposition into CaO and CO2.
[0011] Furthermore, in the iron-rich red mud, the content of Fe2O3 is 30wt%-60wt%, the content of SiO2 is 3wt%-20wt%, the content of Al2O3 is 10wt%-20wt%, the content of CaO is 2wt%-10wt%, the content of Na2O is 2wt%-10wt%, and the content of TiO2 is 0.1wt%-10wt%.
[0012] Furthermore, in the LT dry dust removal ash, the content of TFe is 46wt%-47wt%, the content of CaO is 15wt%-20wt%, the content of SiO2 is 1.2wt%-1.5wt%, the content of Al2O3 is 0wt%-1wt%, the content of MgO is 1wt%-6.5wt%, the content of S is 0.06wt%-0.37wt%, and the remaining components include but are not limited to P, MnO, TiO2, Na2O and K2O. The LT dry dust removal ash is the dust treated by the evaporative cooler + electrostatic precipitator + coal gas cooler system. This kind of dust removal ash has a good slag-forming effect, and the cooling capacity is about 0.85 times that of the ore. It can effectively reduce the consumption of slag-making materials and high-priced cold materials, improve the end point control of the converter, and the return of the LT dry dust removal ash to the furnace can also achieve the maximum recovery of iron elements.
[0013] Furthermore, the limestone has a particle size of 5-15 mm and is dry and free of impurities. Small-particle limestone can be decomposed into CaO and CO2 at a faster rate in molten iron. CaO can increase the basicity of converter slag and reduce the consumption of lime in slag-making material on the one hand, and provide a calcium source for the formation of composite calcium ferrite on the other hand; CO2 can improve the fluidity of pre-melted slag in the ladle and avoid agglomeration and hardening.
[0014] Furthermore, in step 2, the stirring head is lowered to 300-500 mm below the molten iron liquid surface to stir the molten iron for the first time, the rotation speed of the stirring head is 30-50 rpm, and the duration of the first stirring is 3-5 min. The stirring head is preferably a KR stirring head. During the first stirring process, the iron-rich red mud, LT dry dust removal ash, small-grained limestone and the iron slag in the ladle are fully mixed; the rotation speed of the stirring head is controlled at 30-50 rpm, which can avoid dust overflow caused by vigorous stirring and reduce material loss and waste.
[0015] Furthermore, in step 3, the stirring head is lowered to 200-300 mm below the molten iron surface to stir the molten iron for the second time, the rotation speed of the stirring head is 40-60 rpm, and the duration of the second stirring is 1-2 min. During the second stirring process, the iron-rich red mud, LT dry dust removal ash, and small-grained limestone can be further mixed with the iron slag in the ladle to ensure uniform mixing.
[0016] Further, the feeding device includes a high-pressure nitrogen source, which is respectively connected to the air flow inlet of the mixing storage tank, the air flow inlet of the iron ladle and the desulfurizer tank, the feed port of the mixing storage tank is respectively connected to the iron-rich red mud silo, the LT dry dust removal ash silo and the small-grained limestone silo, and the discharge port of the mixing storage tank and the discharge port of the desulfurizer tank are respectively connected to the iron ladle. A mixing bin can be set between the feed port of the mixing storage tank and the iron-rich red mud silo, the LT dry dust removal ash silo and the small-grained limestone silo, and a stirring device is set in the mixing bin. The iron-rich red mud, LT dry dust removal ash and small-grained limestone can first enter the mixing bin for uniform mixing, and then enter the mixing storage tank in the form of a mixed material for storage. The high-pressure nitrogen source can be used as a transport carrier to transport the mixed material or desulfurizer to the iron ladle, or it can directly enter the iron ladle to blow nitrogen into the iron ladle.
[0017] The beneficial effects of the present invention are: The present invention provides a feeding method for absorbing iron-rich red mud in a molten iron pretreatment process, which makes full use of the waiting time from the end of desulfurization to the addition to a converter in the molten iron pretreatment process, and evenly mixes limestone, industrial solid waste iron-rich red mud, and LT dry dust removal ash, and then sprays them into the molten iron with a nitrogen gas flow as a carrier, and then uses the original stirring head in the molten iron pretreatment process to sequentially stir the molten iron for the first time and the second time, so as to promote the limestone, the iron-rich red mud and the LT dry dust removal ash to be evenly dispersed in the molten iron. The limestone, the iron-rich red mud and the LT dry dust removal ash can form a low-melting-point phase of composite calcium ferrite under the heat condition provided by the molten iron, which provides favorable conditions for the recovery of iron resources and valuable minerals in the red mud and the LT dry dust removal ash, and the slag and rapid dephosphorization in the early stage of blowing. At the same time, the composite calcium ferrite covers the slag layer of the molten iron ladle, and can also play a certain heat preservation role, thereby reducing the heat loss of the molten iron and reducing the temperature drop of the molten iron in the pretreatment process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0019] Figure 1 It is a schematic diagram of the connection relationship of the feeding device in Example 1.
[0020] In the figure, 1-iron-rich red mud silo, 2-LT dry dust removal ash silo, 3-small-size limestone silo, 4-first material pipe, 5-second material pipe, 6-third material pipe, 7-mixing bin, 8-fourth material pipe, 9-mixing storage tank, 10-first air flow conveying pipe, 11-second air flow conveying pipe, 12-desulfurizer tank, 13-high-pressure nitrogen source, 14-third air flow conveying pipe, 15-first mixed material conveying pipe, 16-second mixed material conveying pipe, 17-switching valve, 18-discharging chute, 19-iron ladle. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0022] Example 1 A feeding device, such as Figure 1As shown, it includes an iron-rich red mud silo 1, an LT dry dust ash silo 2 and a small-particle limestone silo 3. The discharge port of the iron-rich red mud silo 1, the discharge port of the LT dry dust ash silo 2 and the discharge port of the small-particle limestone silo 3 are respectively connected to the inlet of the mixing silo 7 through the first material pipe 4, the second material pipe 5 and the third material pipe 6. The mixing silo 7 is provided with a mechanical stirring paddle. The outlet of the mixing silo 7 is connected to the feed port of the mixing storage tank 9 through the fourth material pipe 8. The discharge port of the mixing storage tank 9 is connected to the inlet of the switching valve 17 through the first mixing feed pipe 15. The outlet of the switching valve 17 is connected to the molten iron ladle 19 through the discharge chute 18. Among them, the mixing storage tank 9 is provided with an air flow inlet, and the air flow inlet of the mixing storage tank 9 is connected with the high-pressure nitrogen source 13 through the first air flow conveying pipe 10, and the high-pressure nitrogen source 13 is connected with the air flow inlet of the desulfurization agent tank 12 through the second air flow conveying pipe 11, and the discharge port of the desulfurization agent tank 12 is connected with the inlet of the switching valve 17 through the second mixing conveying pipe 16, and the high-pressure nitrogen source 13 is also connected with the inlet of the switching valve 17 through the third air flow conveying pipe 14.
[0023] The discharge port of the iron-rich red mud silo 1, the discharge port of the LT dry dust removal ash silo 2, the discharge port of the small-size limestone silo 3, the outlet of the mixing silo 7, the discharge port of the mixed material storage tank 9, and the discharge port of the desulfurizer tank 12 are respectively provided with discharge gate valves. The first nitrogen shut-off valve, the second nitrogen shut-off valve, and the third nitrogen shut-off valve are respectively provided at the connection between the high-pressure nitrogen source 13 and the first airflow delivery pipe 10, the second airflow delivery pipe 11, and the third airflow delivery pipe 14.
[0024] Example 2 A feeding method for absorbing iron-rich red mud in a molten iron pretreatment process using the feeding device described in Example 1 comprises the following steps: Step 1: Open the discharge gate valve of the iron-rich red mud silo, the discharge gate valve of the LT dry dust ash silo and the discharge gate valve of the small-grained limestone silo, and transport the iron-rich red mud in the iron-rich red mud silo, the LT dry dust ash in the LT dry dust ash silo and the small-grained limestone in the small-grained limestone silo to the mixing silo according to the mass ratio of 4.25:2.15:1, and then use the mechanical stirring paddle in the mixing silo to mix the materials in the mixing silo evenly, and store the obtained mixed materials in the mixing storage tank for standby use. In the iron-rich red mud, the content of Fe2O3 is 30wt%-60wt%, the content of SiO2 is 3wt%-20wt%, the content of Al2O3 is 10wt%-20wt%, the content of CaO is 2wt%-10wt%, the content of Na2O is 2wt%-10wt%, and the content of TiO2 is 0.1wt%-10wt%. In the LT dry dust removal ash, the content of TFe is 46wt%-47wt%, the content of CaO is 15wt%-20wt%, the content of SiO2 is 1.2wt%-1.5wt%, the content of Al2O3 is 0wt%-1wt%, the content of MgO is 6.5wt%, the content of S is 0.06wt%-0.37wt%, and the remaining components include but are not limited to P, MnO, TiO2, Na2O and K2O. The limestone is dry and free of impurities with a particle size of 5-15mm.
[0025] The average amount of mixed material added per ton of steel in this year is G0 = 8.6kg / t, and the average temperature of molten iron in this year is T 经验 =1536℃, the average value of limestone pre-melting time in this year is t 预熔经验 = 8min, the time for limestone to decompose into CaO and CO2 is the average value of the historical furnaces this year t 分解经验 =12min. The molten iron temperature of this batch is T=1362℃, and the average temperature of each batch of molten iron in this shift is T 平均 =1356℃; t 预熔 ,t 分解 8.3min and 12.6min respectively; the sum of the content of Si and P elements in the molten iron of this batch (Si+P) = 0.62wt%; the sum of the content of Si and P elements in the molten steel of each batch in this shift (Si+P) 平均 =0.56wt%, substitute the above parameters into the following formula to calculate the amount of steel added per ton of mixed material G:
[0026]
[0027] ≈9.238kg / t; The amount of molten iron processed in this embodiment is 140t, so the total amount of mixed material added in this batch is G 总 G×140=1293.32kg, G 总 =G 泥 +G 灰 +G 石 , G 泥 is the amount of iron-rich red mud added, G 灰 G is the amount of LT dry dust added 石 is the amount of small-grained limestone added. 泥 : G 灰 : G 石 =4.25:2.15:1, it can be calculated that G 泥 =742.79kg, G 灰 =375.76kg, G 石 =174.77kg.
[0028] The total content of CaO and SiO2 in the mixed material can be calculated by the following formula: [CaO (G 泥 )+CaO(G 灰 )+CaO(G 石 )] / G 总 =23wt%; [SiO2 (G 泥 )+SiO2(G 灰 )+SiO2(G 石 )] / G 总 =2.25wt%; CaO(G 泥 )、CaO(G 灰 )、CaO(G 石 ) are the mass of CaO introduced from iron-rich red mud, LT dry dust removal ash and small-grained limestone in the mixed material, in kg; SiO2 (G 泥 )、SiO2(G 灰 )、SiO2(G 石 ) are the masses of SiO2 introduced into the mixed material from iron-rich red mud, LT dry dust removal ash, and small-grained limestone, respectively, in kg.
[0029] Step 2: Open the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and control the switching valve to open the passage between the desulfurizer tank and the ladle, and use the high-pressure nitrogen flow to spray the desulfurizer in the desulfurizer tank into the molten iron in the ladle, stir and desulfurize, and then skim the slag.
[0030] Step 3: After the slag removal is completed, close the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and at the same time open the discharge gate valve and the first nitrogen shut-off valve of the mixing storage tank, and control the switching valve to open the passage between the mixing storage tank and the molten iron ladle, and use the high-pressure nitrogen gas flow to spray the mixed material in the mixing storage tank into the molten iron, and then slowly lower the KR stirring head to 350mm below the molten iron surface for the first stirring. The speed of the KR stirring head is 40 rpm, and the duration of the first stirring is 3.5min. After the first stirring is completed, lift the KR stirring head to the waiting position and wait for 2min.
[0031] Step 4: Slowly lower the KR stirring head to 250mm below the molten iron surface to stir the molten iron for the second time. The speed of the KR stirring head is 50 rpm. The duration of the second stirring is 2min. After the second stirring is completed, lift the stirring head to the waiting position to obtain molten iron containing pre-molten slag.
[0032] Step 5: Drive the ladle car to the waiting position and wait for the crane to lift it to the converter. Add scrap steel and molten iron containing pre-melted slag into the converter and start blowing. During the blowing process, first lower the oxygen lance to a position where the oxygen lance nozzle is 1000mm away from the molten pool surface, and control the oxygen flow rate to 10000m 3 / h, the time is 3min, and then transfer to normal blowing and corresponding operations.
[0033] The oxygen lance position was adjusted according to the slagging situation, the blowing process was smooth, there were no abnormal conditions such as "splashing" and "drying back", and the steel alloying was normal after the blowing. Compared with the average value of historical furnaces, the amount of active lime added per ton of steel in this furnace was reduced by 0.23kg, the blowing time was shortened by 15 seconds, the phosphorus content at the end of blowing was reduced by 0.002%, and the weight of molten steel increased by 210kg.
[0034] Example 3 A feeding method for absorbing iron-rich red mud in a molten iron pretreatment process using the feeding device described in Example 1 comprises the following steps: Step 1: Open the discharge gate valve of the iron-rich red mud silo, the discharge gate valve of the LT dry dust ash silo and the discharge gate valve of the small-grained limestone silo, and transport the iron-rich red mud in the iron-rich red mud silo, the LT dry dust ash in the LT dry dust ash silo and the small-grained limestone in the small-grained limestone silo to the mixing silo according to the mass ratio of 4.5:2.25:1, and then use the mechanical stirring paddle in the mixing silo to mix the materials in the mixing silo evenly, and store the obtained mixed materials in the mixing storage tank for standby use. In the iron-rich red mud, the content of Fe2O3 is 30wt%-60wt%, the content of SiO2 is 3wt%-20wt%, the content of Al2O3 is 10wt%-20wt%, the content of CaO is 2wt%-10wt%, the content of Na2O is 2wt%-10wt%, and the content of TiO2 is 0.1wt%-10wt%. In the LT dry dust removal ash, the content of TFe is 46wt%-47wt%, the content of CaO is 15wt%-20wt%, the content of SiO2 is 1.2wt%-1.5wt%, the content of Al2O3 is 0wt%-1wt%, the content of MgO is 6.5wt%, the content of S is 0.06wt%-0.37wt%, and the remaining components include but are not limited to P, MnO, TiO2, Na2O and K2O. The limestone is dry and free of impurities with a particle size of 5-15mm.
[0035] The average amount of mixed material added per ton of steel in this year is G0 = 8.6kg / t; the average temperature of molten iron in this year is T 经验 =1536℃, the average value of limestone pre-melting time in this year is t 预熔经验 = 8min, the time for limestone to decompose into CaO and CO2 is the average value of the historical furnaces this year t 分解经验 =12min. The molten iron temperature of this batch is T=1356℃, and the average temperature of each batch of molten iron in this shift is T 平均 =1365℃; t 预熔 ,t 分解 8.1min and 12.3min respectively; the sum of the content of Si and P elements in the molten iron of this batch (Si+P) = 0.58wt%; the sum of the content of Si and P elements in the molten steel of each batch in this shift (Si+P) 平均 =0.55wt%, substitute the above parameters into the following formula to calculate the amount of steel added per ton of mixed material G:
[0036]
[0037] ≈8.254kg / t; The amount of molten iron processed in this embodiment is 142t, so the total amount of mixed material added in this batch is G 总 G×142=1172.068kg, G 总 =G 泥 +G 灰 +G 石 , G 泥 is the amount of iron-rich red mud added, G 灰 G is the amount of LT dry dust added 石 is the amount of small-grained limestone added. 泥 : G 灰 : G 石 =4.5:2.25:1, G can be calculated 泥 : G 灰 : G 石 =4.5:2.25:1=680.56:340.28:151.23, that is, G 泥 =680.56kg, G 灰 =340.28kg, G 石 =151.23kg.
[0038] The total content of CaO and SiO2 in the mixed material can be calculated by the following formula: [CaO (G 泥 )+CaO(G 灰 )+CaO(G 石 )] / G 总 =21wt%; [SiO2 (G 泥 )+SiO2(G 灰 )+SiO2(G 石 )] / G 总 =2.35wt%; CaO(G 泥 )、CaO(G 灰 )、CaO(G 石 ) are the mass of CaO introduced from iron-rich red mud, LT dry dust removal ash and small-grained limestone in the mixed material, in kg; SiO2 (G 泥 )、SiO2(G 灰 )、SiO2(G 石 ) are the masses of SiO2 introduced into the mixed material from iron-rich red mud, LT dry dust removal ash, and small-grained limestone, respectively, in kg.
[0039] Step 2: Open the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and control the switching valve to open the passage between the desulfurizer tank and the ladle, and use the high-pressure nitrogen flow to spray the desulfurizer in the desulfurizer tank into the molten iron in the ladle, stir and desulfurize, and then skim the slag.
[0040] Step 3: After the slag removal is completed, close the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and at the same time open the discharge gate valve and the first nitrogen shut-off valve of the mixing storage tank, and control the switching valve to open the passage between the mixing storage tank and the molten iron ladle, and use the high-pressure nitrogen gas flow to spray the mixed material in the mixing storage tank into the molten iron, and then slowly lower the KR stirring head to 350mm below the molten iron surface for the first stirring. The speed of the KR stirring head is 45 rpm, and the duration of the first stirring is 3.2min. After the first stirring is completed, lift the KR stirring head to the waiting position and wait for 2min.
[0041] Step 4: Slowly lower the KR stirring head to 280mm below the molten iron surface to stir the molten iron for the second time. The speed of the KR stirring head is 40 rpm. The duration of the second stirring is 2min. After the second stirring is completed, lift the stirring head to the waiting position to obtain molten iron containing pre-molten slag.
[0042] Step 5: Drive the ladle car to the waiting position and wait for the crane to lift it to the converter. Add scrap steel and molten iron containing pre-melted slag into the converter and start blowing. During the blowing process, first lower the oxygen lance to a position where the oxygen lance nozzle is 1000mm away from the molten pool surface, and control the oxygen flow rate to 10000m 3 / h, the time is 2.5min, and then transfer to normal blowing and corresponding operations.
[0043] The oxygen lance position was adjusted according to the slagging situation, the blowing process was smooth, there were no abnormal conditions such as "splashing" and "drying back", and the steel alloying was normal after the blowing. Compared with the average value of historical furnaces, the amount of active lime added per ton of steel in this furnace was reduced by 0.18kg, the blowing time was shortened by 12 seconds, the phosphorus content at the end of blowing was reduced by 0.002%, and the weight of molten steel increased by 170kg.
[0044] Comparative Example 1 A feeding method for absorbing iron-rich red mud in a molten iron pretreatment process using the feeding device described in Example 1 comprises the following steps: Step 1: Open the discharge gate valve of the iron-rich red mud silo, the discharge gate valve of the LT dry dust ash silo and the discharge gate valve of the small-grained limestone silo, and transport the iron-rich red mud in the iron-rich red mud silo, the LT dry dust ash in the LT dry dust ash silo and the small-grained limestone in the small-grained limestone silo to the mixing silo according to the mass ratio of 3.5:2.0:1, and then use the mechanical stirring paddle in the mixing silo to mix the materials in the mixing silo evenly, and store the obtained mixed materials in the mixing storage tank for standby use. In the iron-rich red mud, the content of Fe2O3 is 30wt%-60wt%, the content of SiO2 is 3wt%-20wt%, the content of Al2O3 is 10wt%-20wt%, the content of CaO is 2wt%-10wt%, the content of Na2O is 2wt%-10wt%, and the content of TiO2 is 0.1wt%-10wt%. In the LT dry dust removal ash, the content of TFe is 46wt%-47wt%, the content of CaO is 15wt%-20wt%, the content of SiO2 is 1.2wt%-1.5wt%, the content of Al2O3 is 0wt%-1wt%, the content of MgO is 6.5wt%, the content of S is 0.06wt%-0.37wt%, and the remaining components include but are not limited to P, MnO, TiO2, Na2O and K2O. The limestone is dry and free of impurities with a particle size of 5-15mm.
[0045] The average amount of mixed material added per ton of steel in this year is G0 = 8.6kg / t, and the average temperature of molten iron in this year is T 经验 =1536℃, the average value of limestone pre-melting time in this year is t 预熔经验 = 8min, the time for limestone to decompose into CaO and CO2 is the average value of the historical furnaces this year t 分解经验 =12min. The molten iron temperature of this batch is T=1376℃, and the average temperature of each batch of molten iron in this shift is T 平均 =1365℃; the sum of the content of Si and P in the molten iron of this batch (Si+P) = 0.58wt%; the sum of the content of Si and P in the molten steel of each batch in this shift (Si+P) 平均 =0.55wt%, the molten iron temperature of this batch T, the average temperature of each batch of molten iron in this shift T 平均 , the sum of the Si and P contents in the molten iron of this heat (Si+P) and the sum of the Si and P contents in the molten steel of each heat in this shift (Si+P) 平均 Substitute the following formula to calculate the amount of steel added per ton of mixed material G:
[0046]
[0047] ≈8.50kg / t; The amount of molten iron processed in this embodiment is 142t, so the total amount of mixed material added in this batch is G 总 G×142=1207kg, G 总 =G 泥 +G 灰 +G 石 , G 泥 is the amount of iron-rich red mud added, G 灰 G is the amount of LT dry dust added 石 is the amount of small-grained limestone added. 泥 : G 灰 : G 石 =3.5:2.0:1, G can be calculated 泥 : G 灰 : G 石 =3.5:2.0:1=649.92:371.38:185.69, that is, G 泥 =649.92kg, G 灰 =371.38kg, G 石 =185.69kg.
[0048] The total content of CaO and SiO2 in the mixed material can be calculated by the following formula: [CaO (G 泥 )+CaO(G 灰 )+CaO(G 石 )] / G 总 =21wt%; [SiO2 (G 泥 )+SiO2(G 灰 )+SiO2(G 石 )] / G 总 =2.35wt%; CaO(G 泥 )、CaO(G 灰 )、CaO(G 石 ) are the mass of CaO introduced from iron-rich red mud, LT dry dust removal ash and small-grained limestone in the mixed material, in kg; SiO2 (G 泥 )、SiO2(G 灰 )、SiO2(G 石 ) are the masses of SiO2 introduced into the mixed material from iron-rich red mud, LT dry dust removal ash, and small-grained limestone, respectively, in kg.
[0049] Step 2: Open the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and control the switching valve to open the passage between the desulfurizer tank and the ladle, and use the high-pressure nitrogen flow to spray the desulfurizer in the desulfurizer tank into the molten iron in the ladle, stir and desulfurize, and then skim the slag.
[0050] Step 3: After the slag removal is completed, close the discharge gate valve and the second nitrogen shut-off valve of the desulfurizer silo, and at the same time close the discharge gate valve and the first nitrogen shut-off valve of the mixing storage tank, and control the switching valve to open the passage between the mixing storage tank and the molten iron ladle, and use the high-pressure nitrogen gas flow to spray the mixed material in the mixing storage tank into the molten iron, and then slowly lower the KR stirring head to 350mm below the molten iron surface for the first stirring. The speed of the KR stirring head is 45 rpm, and the duration of the first stirring is 3.2min. After the first stirring is completed, lift the KR stirring head to the waiting position and wait for 2min.
[0051] Step 4: Slowly lower the KR stirring head to 280mm below the molten iron surface to stir the molten iron for the second time. The speed of the KR stirring head is 40 rpm. The duration of the second stirring is 2min. After the second stirring is completed, lift the stirring head to the waiting position to obtain molten iron containing pre-molten slag.
[0052] Step 5: Drive the ladle car to the waiting position and wait for the crane to lift it to the converter. Add scrap steel and molten iron containing pre-melted slag into the converter and start blowing. During the blowing process, first lower the oxygen lance to a position where the oxygen lance nozzle is 1000mm away from the molten pool surface, and control the oxygen flow rate to 10000m 3 / h, the time is 2.5min, and then transfer to normal blowing and corresponding operations.
[0053] The oxygen lance position was adjusted according to the slagging situation, the blowing process was smooth, there were no abnormal conditions such as "splashing" and "drying back", and the steel alloying was normal after the blowing. Compared with the average value of historical furnaces, the amount of active lime added per ton of steel in this furnace was reduced by 0.01kg, the blowing time was shortened by 1 second, the phosphorus content at the end of blowing was reduced by 0.001%, and the weight of molten steel increased by 30kg.
[0054] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.
Claims
1. A method for feeding iron-rich red mud in a molten iron pretreatment process, characterized in that: The steps include: Step 1: using a feeding device to evenly mix the iron-rich red mud, LT dry dust removal ash and limestone to obtain a mixed material; Step 2: Spray the mixed material into the molten iron using a nitrogen gas flow, lower the stirring head to stir the molten iron for the first time, and after the first stirring is completed, lift the stirring head to the waiting position; Step 3: lower the stirring head to stir the molten iron for the second time. After the second stirring is completed, lift the stirring head to the waiting position; Step 4: Transport the molten iron to the converter, add scrap steel and then blow it.
2. The feeding method according to claim 1, characterized in that In the mixed material, the mass ratio of iron-rich red mud, LT dry dust removal ash and limestone is 4-5:2-2.5:
1.
3. The feeding method according to claim 2, characterized in that In the mixed material, the total content of CaO is 15wt%-25wt%; the total content of SiO2 is 2wt%-2.5wt%.
4. The feeding method according to claim 1, characterized in that In step 2, the amount of mixed material added per ton of steel is calculated according to the following formula: , G is the amount of steel added per ton of mixed material, in kg / t; G0 is the historical average of the amount of mixed material added per ton of steel in the current year, in kg / t; T is the temperature of the molten iron in this batch, in °C; T 平均 The average temperature of molten iron in each furnace in this shift, in °C; (Si+P) is the sum of the contents of Si and P in the molten iron of this batch, in wt%; (Si+P) 平均 It is the average value of the sum of the contents of Si and P in each heat of molten steel in this shift, in wt%; T 经验 The average value of molten iron temperature in the current year, in °C; t 预熔 is the pre-melting time of limestone, in min, t 预熔经验 The average value of limestone pre-melting time in the current year, in minutes; t 分解 The theoretical calculation time for limestone to decompose into CaO and CO2, in min, t 分解经验 It is the historical average time of limestone decomposition into CaO and CO2 this year, in minutes.
5. The feeding method according to claim 1, characterized in that: In the iron-rich red mud, the content of Fe2O3 is 30wt%-60wt%, the content of SiO2 is 3wt%-20wt%, the content of Al2O3 is 10wt%-20wt%, the content of CaO is 2wt%-10wt%, the content of Na2O is 2wt%-10wt%, and the content of TiO2 is 0.1wt%-10wt%.
6. The feeding method according to claim 1, characterized in that: In the LT dry dust removal ash, the TFe content is 46wt%-47wt%, the CaO content is 15wt%-20wt%, the SiO2 content is 1.2wt%-1.5wt%, the Al2O3 content is 0wt%-1wt%, the MgO content is 1wt%-6.5wt%, and the S content is 0.06wt%-0.37wt%.
7. The feeding method according to claim 1, characterized in that The particle size of limestone is 5-15mm.
8. The feeding method according to claim 1, characterized in that In step 2, the stirring head is lowered to 300-500 mm below the molten iron surface to stir the molten iron for the first time. The rotation speed of the stirring head is 30-50 rpm, and the duration of the first stirring is 3-5 minutes.
9. The feeding method according to claim 1, characterized in that: In step three, the stirring head is lowered to 200-300 mm below the molten iron surface to stir the molten iron for the second time. The rotation speed of the stirring head is 40-60 rpm, and the duration of the second stirring is 1-2 min.
10. The feeding method according to any one of claims 1 to 9, characterized in that: The feeding device includes a high-pressure nitrogen source, which is respectively connected to the air flow inlet of the mixing storage tank, the air flow inlet of the molten iron ladle and the desulfurizer tank; the feed port of the mixing storage tank is respectively connected to the iron-rich red mud silo, the LT dry dust removal ash silo and the small-particle limestone silo; the discharge port of the mixing storage tank and the discharge port of the desulfurizer tank are respectively connected to the molten iron ladle.
Citation Information
Patent Citations
Desulfuration slagging agent
CN107312909A
Molten iron desiliconization agent using electric precipitation dust of sintering head as substrate
CN108220529A
Recycling method of iron-rich red mud in iron and steel industry
CN116377159A
Method for co-processing iron-rich red mud, converter dedusting ash and refining slag in steelmaking process
CN116891923A