Corrosion-resistant foundation bolt

By optimizing the elemental composition and phosphating treatment of anchor bolts, especially by using a composite phosphating solution of modified montmorillonite, the problems of insufficient corrosion resistance and tensile strength of anchor bolts have been solved, achieving higher corrosion resistance and tensile strength.

CN119040765AActive Publication Date: 2024-11-29HEBEI XINTU FASTENER MANUFACTURING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411222116.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-29
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing anchor bolts have poor corrosion resistance and tensile strength, making it difficult to meet the requirements of harsh service environments.

Method used

The billet is made of specific elements and then subjected to phosphate treatment after cold heading and threading. The corrosion resistance and tensile strength of the anchor bolts are improved by using composite phosphate solution and modified montmorillonite. This includes optimizing the ratio of Al, Zr and Nb, and adding montmorillonite and modified montmorillonite to the phosphate solution.

Benefits of technology

It significantly improves the tensile strength and corrosion resistance of anchor bolts, meeting the needs of practical engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of fasteners, and provides a corrosion-resistant foundation bolt which is obtained by carrying out cold heading, thread machining and phosphating treatment on a blank, and the blank is prepared from the following components in percentage by weight: 0.33%-0.51% of C, 0.4%-0.7% of Mn, 1.3%-2.5% of Cr, 1.2%-4.8% of Al, 1.2%-4.9% of Zr, 2.8%-4.8% of Nb, less than or equal to 0.015% of P, less than or equal to 0.01% of S and the balance of Fe and other inevitable impurities. According to the technical scheme, the problem that the corrosion resistance and the tensile strength of a foundation bolt in the related technology are poor is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fasteners, and in particular to corrosion-resistant anchor bolts. Background Art

[0002] With the acceleration of industrial modernization and the continuous advancement of technology, anchor bolts, as important mechanical equipment fixing components, play a key role in various engineering projects. Anchor bolts are not only widely used in traditional industrial facilities, such as equipment installation in the power, chemical, manufacturing and other industries, but also in the emerging clean energy field, such as photovoltaic power generation, wind power generation and other power station construction. It also plays an indispensable role.

[0003] The corrosion resistance and tensile strength of anchor bolts directly affect the stability of mechanical equipment. As the service environment of anchor bolts becomes increasingly harsh, the market has put forward more stringent requirements on their corrosion resistance and tensile strength. Therefore, the research and development of new anchor bolts is of great significance for practical engineering applications. Summary of the invention

[0004] The present invention provides a corrosion-resistant anchor bolt, which solves the problem of poor corrosion resistance and tensile strength of the anchor bolt in the related art.

[0005] The technical solution of the present invention is as follows: The invention provides a corrosion-resistant anchor bolt, which is obtained by cold heading, thread processing and phosphating treatment of a blank, wherein the blank consists of the following components in weight percentage: C 0.33%-0.51%, Mn 0.4%-0.7%, Cr 1.3%-2.5%, Al 1.2%-4.8%, Zr 1.2%-4.9%, Nb 2.8%-4.8%, P≤0.015%, S≤0.01%, and the rest is Fe and other inevitable impurities.

[0006] As a further technical solution, during the phosphating treatment, the phosphating solution includes the following components in parts by weight: 80-100 parts of phosphoric acid, 40-60 parts of zinc nitrate, 30-50 parts of manganese nitrate, 30-50 parts of zinc dihydrogen phosphate, and 1000 parts of water.

[0007] As a further technical solution, the ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2.

[0008] In the present invention, when the ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2, it helps to further improve the tensile strength of the anchor bolt.

[0009] As a further technical solution, the weight of the Al is greater than the weight of the Zr.

[0010] In the present invention, when the ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2 and the weight of Al is greater than the weight of Zr, it helps to further improve the tensile strength of the anchor bolt.

[0011] As a further technical solution, during the phosphating treatment, the phosphating solution includes the following components in parts by weight: 80-100 parts of phosphoric acid, 40-60 parts of zinc nitrate, 30-50 parts of manganese nitrate, 30-50 parts of zinc dihydrogen phosphate, 5-9.5 parts of montmorillonite, and 1000 parts of water.

[0012] In the present invention, the composite phosphating system is used for phosphating treatment, which is beneficial to further improve the corrosion resistance of the anchor bolts. The montmorillonite in the phosphating solution can be adsorbed on the surface of the blank to promote the formation of phosphate crystals; on the other hand, it can be filled in the pores of the phosphate film layer to form a denser phosphating film, thereby further improving the corrosion resistance of the anchor bolts.

[0013] As a further technical solution, the particle size of the montmorillonite is 1000-2000 mesh.

[0014] As a further technical solution, the montmorillonite is modified montmorillonite, and the modified montmorillonite includes the following components: montmorillonite, ammonium ferric citrate and cupric chloride.

[0015] In the present invention, the corrosion resistance of the anchor bolts is further improved by modifying the montmorillonite with ammonium ferric citrate and cupric chloride. It is speculated that this is because the cation exchange capacity of the modified montmorillonite is further improved, thereby further promoting the formation of phosphate crystals and making the phosphate film denser.

[0016] As a further technical solution, in the modified montmorillonite, the weight ratio of the montmorillonite to ammonium ferric citrate and cupric chloride is 90:3-8:2.

[0017] In the present invention, when the weight ratio of montmorillonite to ammonium ferric citrate and cupric chloride in the modified montmorillonite is 90:3-8:2, it helps to further improve the corrosion resistance of the anchor bolts.

[0018] As a further technical solution, the preparation method of the modified montmorillonite comprises the following steps: dispersing montmorillonite in water, adjusting the pH value to 6-6.5, adding ammonium ferric citrate and copper chloride, mixing evenly, reacting, filtering, and obtaining the modified montmorillonite.

[0019] As a further technical solution, during the reaction, the temperature is 60-80°C and the time is 2-3h.

[0020] The present invention also provides a method for preparing the corrosion-resistant anchor bolt, comprising the following steps: the blank is subjected to cold heading, thread processing and phosphating treatment to obtain the anchor bolt.

[0021] As a further technical solution, during the phosphating treatment, the temperature is 40-50°C and the time is 20-30 minutes.

[0022] The working principle and beneficial effects of the present invention are: In the present invention, the element composition of the anchor bolt blank is optimized to give full play to the synergistic effect between the elements, and phosphating treatment is performed, so that the anchor bolt has good corrosion resistance and tensile strength, which can meet the needs of practical engineering applications. In particular, the tensile strength of the anchor bolt is significantly improved through the combined effect of Al, Zr and Nb. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the following examples and comparative examples, unless otherwise specified, the blanks were cast using a conventional casting process, and the particle size of the montmorillonite was 1500 meshes.

[0025] Example 1 The preparation method of the corrosion-resistant anchor bolt comprises the following steps: cold heading, thread processing and phosphating treatment of the blank to obtain the anchor bolt; The blank is composed of the following components in weight percentage: C 0.33%, Mn 0.4%, Cr 1.3%, Al 1.2%, Zr 1.2%, Nb 2.8%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities; During the phosphating treatment, the temperature is 40° C., the time is 30 minutes, and the phosphating solution includes the following components in parts by weight: 80 parts of phosphoric acid, 40 parts of zinc nitrate, 30 parts of manganese nitrate, 30 parts of zinc dihydrogen phosphate, and 1000 parts of water.

[0026] Example 2 The preparation method of the corrosion-resistant anchor bolt comprises the following steps: cold heading, thread processing and phosphating treatment of the blank to obtain the anchor bolt; The blank is composed of the following components in weight percentage: C 0.51%, Mn 0.7%, Cr 2.5%, Al 4.8%, Zr 4.9%, Nb 4.8%, P 0.01%, S 0.005%, and the rest is Fe and other inevitable impurities; During the phosphating treatment, the temperature is 50° C., the time is 20 minutes, and the phosphating solution includes the following components in parts by weight: 100 parts of phosphoric acid, 60 parts of zinc nitrate, 50 parts of manganese nitrate, 50 parts of zinc dihydrogen phosphate, and 1000 parts of water.

[0027] Example 3 The preparation method of the corrosion-resistant anchor bolt comprises the following steps: cold heading, thread processing and phosphating treatment of the blank to obtain the anchor bolt; The blank is composed of the following components in weight percentage: C 0.41%, Mn 0.55%, Cr 1.8%, Al 1.8%, Zr 2.4%, Nb 4.8%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities; During the phosphating treatment, the temperature is 45° C., the time is 25 minutes, and the phosphating solution includes the following components in parts by weight: 80 parts of phosphoric acid, 40 parts of zinc nitrate, 30 parts of manganese nitrate, 30 parts of zinc dihydrogen phosphate, and 1000 parts of water.

[0028] Example 4 The only difference between this embodiment and embodiment 3 is that in this embodiment, the blank is composed of the following components in weight percentage: C 0.41%, Mn 0.55%, Cr 1.8%, Al 2.7%, Zr 3.5%, Nb 2.8%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0029] Example 5 The only difference between this embodiment and embodiment 3 is that in this embodiment, the blank is composed of the following components in weight percentage: C 0.41%, Mn 0.55%, Cr 1.8%, Al 2%, Zr 2.5%, Nb 4.5%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0030] Example 6 The only difference between this embodiment and embodiment 3 is that in this embodiment, the blank is composed of the following components in weight percentage: C 0.41%, Mn 0.55%, Cr 1.8%, Al 2%, Zr 4%, Nb 3%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0031] Example 7 The only difference between this embodiment and Embodiment 6 is that, in this embodiment, the weight percentage of Al in the blank is 3%, and the weight percentage of Zr is 3%.

[0032] Example 8 The only difference between this embodiment and embodiment 6 is that, in this embodiment, the weight percentage of Al in the blank is 4%, and the weight percentage of Zr is 2%.

[0033] Example 9 The only difference between this embodiment and embodiment 3 is that in this embodiment, the phosphating solution includes the following components in parts by weight: 80 parts of phosphoric acid, 40 parts of zinc nitrate, 30 parts of manganese nitrate, 30 parts of zinc dihydrogen phosphate, 5 parts of montmorillonite, and 1000 parts of water.

[0034] Example 10 The only difference between this embodiment and embodiment 3 is that, in this embodiment, the phosphating solution includes the following components in parts by weight: 100 parts of phosphoric acid, 60 parts of zinc nitrate, 50 parts of manganese nitrate, 50 parts of zinc dihydrogen phosphate, 9.5 parts of montmorillonite, and 1000 parts of water.

[0035] Embodiment 11 The only difference between this embodiment and embodiment 10 is that in this embodiment, the montmorillonite is modified montmorillonite, and the preparation method of the modified montmorillonite includes the following steps: dispersing 8.1 parts of montmorillonite in 100 parts of water, adjusting the pH value to 6.5, adding 1.4 parts of ammonium ferric citrate, mixing evenly, reacting at 70°C for 2.5 hours, filtering, and obtaining modified montmorillonite.

[0036] Example 12 The only difference between this embodiment and embodiment 11 is that in this embodiment, the preparation method of modified montmorillonite includes the following steps: dispersing 8.1 parts of montmorillonite in 100 parts of water, adjusting the pH value to 6.5, adding 1.4 parts of copper chloride, mixing evenly, reacting at 70°C for 2.5 hours, filtering, and obtaining modified montmorillonite.

[0037] Embodiment 13 The only difference between this embodiment and embodiment 11 is that in this embodiment, the preparation method of modified montmorillonite includes the following steps: dispersing 8.1 parts of montmorillonite in 100 parts of water, adjusting the pH value to 6.5, adding 1.22 parts of ammonium ferric citrate and 0.18 parts of cupric chloride, mixing evenly, reacting at 70°C for 2.5 hours, filtering, and obtaining modified montmorillonite.

[0038] Embodiment 14 The only difference between this embodiment and embodiment 11 is that in this embodiment, when preparing modified montmorillonite, the weight part of montmorillonite is 9.24 parts, the weight part of ammonium ferric citrate is 0.05 parts, and the weight part of cupric chloride is 0.21 parts.

[0039] Embodiment 15 The only difference between this embodiment and embodiment 11 is that in this embodiment, when preparing modified montmorillonite, the weight part of montmorillonite is 8.55 parts, the weight part of ammonium ferric citrate is 0.76 parts, and the weight part of cupric chloride is 0.19 parts.

[0040] Example 16 The only difference between this embodiment and embodiment 11 is that in this embodiment, when preparing modified montmorillonite, the weight part of montmorillonite is 9 parts, the weight part of ammonium ferric citrate is 0.3 parts, and the weight part of cupric chloride is 0.2 parts.

[0041] Comparative Example 1 The only difference between this comparative example and Example 1 is that, in this comparative example, the blank is composed of the following components in weight percentage: C 0.33%, Mn 0.4%, Cr 1.3%, Al 2.4%, Nb 2.8%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0042] Comparative Example 2 The only difference between this comparative example and Example 1 is that, in this comparative example, the blank is composed of the following components in weight percentage: C 0.33%, Mn 0.4%, Cr 1.3%, Zr 2.4%, Nb 2.8%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0043] Comparative Example 3 The only difference between this comparative example and Example 1 is that, in this comparative example, the blank is composed of the following components in weight percentage: C 0.33%, Mn 0.4%, Cr 1.3%, Al 2.6%, Zr 2.6%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0044] Comparative Example 4 The only difference between this comparative example and Example 1 is that, in this comparative example, the blank is composed of the following components in weight percentage: C 0.33%, Mn 0.4%, Cr 1.3%, Nb 5.2%, P 0.015%, S 0.01%, and the rest is Fe and other inevitable impurities.

[0045] Experimental Example 1 Tensile Strength Test The tensile strength test of the blanks in Examples 1 to 8 and Comparative Examples 1 to 4 was carried out according to GB / T 228.1-2021 "Tensile test of metallic materials - Part 1: Room temperature test method", wherein the test rate was 0.005s -1 The test results are shown in Table 1 below.

[0046] Table 1 Tensile strength test results

[0047] The comparison between Example 1 and Comparative Examples 1 to 4 shows that by optimizing the elemental composition of the anchor bolt blank, the synergistic effect between the elements is fully utilized, especially through the joint action of Al, Zr and Nb, the tensile strength of the anchor bolt is significantly improved. The comparison between Examples 3 to 4 and Examples 5 to 8 shows that when the ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2, it helps to further improve the tensile strength of the anchor bolt. The comparison between Example 8 and Examples 6 to 7 shows that when the ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2 and the weight of Al is greater than the weight of Zr, it helps to further improve the tensile strength of the anchor bolt.

[0048] Experimental Example 2 Corrosion Resistance Test The anchor bolts prepared in Examples 3 and 9 to 16 were tested for corrosion resistance according to the neutral salt spray test method in GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", and the time when corrosion began to occur was recorded, wherein the test temperature was 35°C, the concentration of the sodium chloride solution was 50 g / L, and the pH value of the collected solution was 7. The test results are shown in Table 2 below.

[0049] Table 2 Corrosion resistance test results

[0050] Comparison between Example 3 and Example 9 shows that by adding montmorillonite to the phosphating solution to form a composite phosphating system, the corrosion resistance of the anchor bolts can be further improved. Comparison between Examples 10-12 and Example 13 shows that by modifying montmorillonite with ammonium ferric citrate and cupric chloride, the corrosion resistance of the anchor bolts can be further improved. Comparison between Examples 13-14 and Examples 15-16 shows that when the weight ratio of montmorillonite to ammonium ferric citrate and cupric chloride in the modified montmorillonite is 90:3-8:2, it helps to further improve the corrosion resistance of the anchor bolts.

[0051] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Corrosion-resistant anchor bolts are obtained by cold heading, thread processing and phosphating of the blank. It is characterized in that The blank is composed of the following components in weight percentage: C 0.33%-0.51%, Mn 0.4%-0.7%, Cr 1.3%-2.5%, Al 1.2%-4.8%, Zr 1.2%-4.9%, Nb 2.8%-4.8%, P≤0.015%, S≤0.01%, and the rest is Fe and other inevitable impurities.

2. The corrosion-resistant anchor bolt according to claim 1, It is characterized in that The ratio of the sum of the weights of Al and Zr to the weight of Nb is 1≤(Al+Zr) / Nb≤2.

3. The corrosion-resistant anchor bolt according to claim 2, It is characterized in that The weight of the Al is greater than the weight of the Zr.

4. The corrosion-resistant anchor bolt according to claim 1, It is characterized in that During the phosphating treatment, the phosphating solution includes the following components in parts by weight: 80-100 parts of phosphoric acid, 40-60 parts of zinc nitrate, 30-50 parts of manganese nitrate, 30-50 parts of zinc dihydrogen phosphate, 5-9.5 parts of montmorillonite, and 1000 parts of water.

5. The corrosion-resistant anchor bolt according to claim 4, It is characterized in that The montmorillonite is modified montmorillonite, and the modified montmorillonite comprises the following components: montmorillonite, ammonium ferric citrate and cupric chloride.

6. The corrosion-resistant anchor bolt according to claim 5, It is characterized in that In the modified montmorillonite, the weight ratio of the montmorillonite to ammonium ferric citrate and copper chloride is 90:3-8:

2.

7. The corrosion-resistant anchor bolt according to claim 5, It is characterized in that The preparation method of the modified montmorillonite comprises the following steps: dispersing montmorillonite in water, adjusting the pH value to 6-6.5, adding ammonium ferric citrate and copper chloride, mixing evenly, reacting, filtering, and obtaining the modified montmorillonite.

8. The corrosion-resistant anchor bolt according to claim 7, It is characterized in that During the reaction, the temperature is 60-80° C. and the reaction time is 2-3 hours.

9. The method for preparing the corrosion-resistant anchor bolt according to any one of claims 1 to 8, It is characterized in that The following steps are involved: The blank is subjected to cold heading, thread processing and phosphating treatment to obtain the anchor bolt.

10. The method for preparing the corrosion-resistant anchor bolt according to claim 9, It is characterized in that During the phosphating treatment, the temperature is 40-50° C. and the time is 20-30 minutes.

Citation Information

Patent Citations

  • Phospahte coated stainless steel wire for cold heading and self-drilling screw using the stainless steel wire

    CN101255589A

  • Preparation method of high-strength anti-corrosion bolt

    CN103088271A

  • Methods for treating a ferrous metal substrate

    CN105026615A

  • Phosphating solution and preparation method thereof

    CN113621953A

  • High-strength member, method for manufacturing high-strength member, and method for manufacturing steel sheet for high-strength member

    CN113840934A