Metal thin layer structure for surface bonding and preparation method
By using surface bonding technology of WTi mixed metal, Au metal, Ni metal, WTi mixed metal and Au metal multi-layer structure on the upper plate of the capacitor, the Ni/Pd/Au plating structure is solved in the preparation of the upper plate of the capacitor. The problems of poor adhesion and excessive stress achieve the effects of high adhesion and high bond tensile strength.
Patent Information
- Application Number
- CN202411174242.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
During the preparation of the capacitor upper plate, the Ni/Pd/Au coating structure has problems such as poor adhesion and excessive stress leading to tearing and disengagement of edge capacitor dielectrics, and is prone to rupture or disengagement after verification of high-strength reliability.
The thin metal structures prepared successively by WTi mixed metal, Au metal, Ni metal, WTi mixed metal, Au metal, and Au metal are formed by magnetron sputtering and electroplating processes, and are carried out by photolithography and wet process. Remove glue and remove excess metal layers to form a surface bonding structure with high adhesion and high bond tensile strength.
The thin metal layer structure with high adhesion and high bond tensile strength is achieved, which can maintain excellent performance after high strength reliability tests, avoiding the problems of metal disengagement of the upper plate and tearing of the capacitor dielectric.
Smart Images

Figure CN119040825A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a metal thin layer structure for surface bonding and a preparation method thereof. Background Art
[0002] With the rapid development of modern wireless communication technology, GaN microwave power devices have been widely studied and applied. Passive devices such as inductors, capacitors, and thin-film resistors, as key components of microwave matching circuits, have also become an important research hotspot.
[0003] The Ni / Pd / Au coating structure has been widely used in the packaging field and can meet the requirements of wire bonding and welding assembly at the same time. However, when the structure is introduced into the preparation process of the upper plate of the capacitor, there are multiple problems. First, Ni cannot be tightly combined with the capacitor dielectric, which easily generates the risk of the upper plate metal being detached; second, the upper plate of the capacitor prepared by the Ni / Pd / Au coating has excessive stress, which easily causes the capacitor dielectric at the edge of the upper plate to tear, the capacitor dielectric is detached from the lower plate, and the device has no capacitance characteristics; third, the capacitor device prepared by the Ni / Pd / Au coating will break or detach from the capacitor dielectric when it undergoes reliability verification such as high storage and temperature cycle. Therefore, it is necessary to provide a new type of metal thin layer structure and preparation method for surface bonding to solve the above-mentioned problems. Summary of the invention
[0004] Purpose of the invention: In order to solve the above problems, the present invention provides a metal thin layer structure for surface bonding and a preparation method. The above metal thin layer structure is used as the upper plate of the capacitor, which has high adhesion and high bonding tensile strength, and can still maintain excellent performance after undergoing high-intensity reliability tests.
[0005] Technical solution: To achieve the above-mentioned purpose, a metal thin layer structure for surface bonding described in the present invention includes a first metal layer, a second metal layer arranged on the first metal layer, a third metal layer arranged on the second metal layer, a fourth metal layer arranged on the third metal layer, a fifth metal layer arranged on the fourth metal layer, and a sixth metal layer arranged on the fifth metal layer; the first metal layer is a WTi mixed metal, the second metal layer is an Au metal, the third metal layer is a Ni metal, the fourth metal layer is a WTi mixed metal, the fifth metal layer is an Au metal, and the sixth metal layer is an Au metal.
[0006] A method for preparing a metal thin layer structure for surface bonding according to claim 1, characterized in that it comprises the following steps:
[0007] S1. The first metal layer is prepared by using a WTi mixed metal target and a magnetron sputtering process;
[0008] S2. The second metal layer is prepared by using Au metal target and magnetron sputtering process;
[0009] S3. The photoresist is coated and cured by a photolithography process in the area where the third metal layer is not required, and the area where the third metal layer needs to be prepared is exposed;
[0010] S4. The third metal layer is prepared by using a Ni metal target and an electroplating process;
[0011] S5. The fourth metal layer is prepared by using a WTi mixed metal target and a magnetron sputtering process;
[0012] S6. The fifth metal layer is prepared by using an Au metal target and a magnetron sputtering process;
[0013] S7. The sixth metal layer is prepared by using an Au metal target and a photoplating process;
[0014] S8. stripping the photoresist;
[0015] S9. Remove the redundant second metal layer and the first metal layer below the area without the third metal layer through a wet process.
[0016] Furthermore, the mass ratio of W metal to Ti metal in the WTi mixed metal target is 2:8 to 5:5.
[0017] Furthermore, in S1, a capacitor dielectric is prepared, and a first metal layer is formed on the surface of the capacitor dielectric by a magnetron sputtering process.
[0018] Furthermore, the first metal layer is used as a seed layer, and the second metal layer is used as a seed layer for electroplating the third metal layer.
[0019] Furthermore, in S8, while removing the photoresist, the third metal layer, the fourth metal layer, the fifth metal layer, and the sixth metal layer on the photoresist are stripped along with the photoresist.
[0020] Furthermore, the sixth metal layer serves as a gold wire bonding layer.
[0021] Furthermore, the thickness of the first metal layer (1) is 40 to 150 nm, the thickness of the second metal layer (2) is 20 to 160 nm, the thickness of the third metal layer (3) is 350 to 1300 nm, the thickness of the fourth metal layer (4) is 40 to 150 nm, the thickness of the fifth metal layer (5) is 20 to 160 nm, and the thickness of the sixth metal layer (6) is 1.1 to 5 μm.
[0022] Furthermore, in S9, when a wet process is used to remove excess metal layer 2 below the area without metal layer 3, the wet solution used is a mixture of potassium cyanide: 647 gold removal concentrate: water in a volume ratio of 1:5:200; when a wet process is used to remove excess metal layer 1 below the area without metal layer 3, the wet solution used is hydrogen peroxide, the temperature is 60°C, and the concentration is 26%.
[0023] Furthermore, the purity of the Au metal target is higher than 99.999%.
[0024] Beneficial effects: Compared with the prior art, the present invention has the following significant effects: a metal thin layer structure prepared in sequence of WTi mixed metal, Au metal, Ni metal, WTi mixed metal, Au metal, and Au metal is used as the upper plate of the capacitor, which has high adhesion and high bonding tensile strength, and can still maintain excellent performance after undergoing high-intensity reliability tests. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the structure of the present invention.
[0026] Figure 2 This is a schematic diagram of the location of the first metal layer of the present invention.
[0027] Figure 3 This is a schematic diagram of the location of the photoresist described in the present invention.
[0028] Figure 4 This is a schematic diagram of the location of the second metal layer of the present invention.
[0029] Figure 5 This is a schematic diagram of the location of the third metal layer described in the present invention.
[0030] Figure 6 This is a schematic diagram of the location of the fourth metal layer described in the present invention.
[0031] Figure 7 This is a schematic diagram of the location of the fifth metal layer described in the present invention.
[0032] Figure 8 This is a schematic diagram of the location of the sixth metal layer described in the present invention.
[0033] Fig. 9 This is a schematic diagram of the overall structure when the redundant metal layer is not removed according to the present invention. DETAILED DESCRIPTION
[0034] The present invention discloses a metal thin layer structure for surface bonding and a preparation method thereof. Figure 1As shown, the metal thin layer structure for surface bonding provided by the present invention is further described in detail below: the metal thin layer structure for surface bonding includes a first metal layer 1, a second metal layer 2 arranged on the first metal layer 1, a third metal layer 3 arranged on the second metal layer 2, a fourth metal layer 4 arranged on the third metal layer 3, a fifth metal layer 5 arranged on the fourth metal layer 4, and a sixth metal layer 6 arranged on the fifth metal layer 5; the first metal layer 1 is a WTi mixed metal, the second metal layer 2 is an Au metal, the third metal layer 3 is a Ni metal, the fourth metal layer 4 is a WTi mixed metal, the fifth metal layer 5 is an Au metal, and the sixth metal layer 6 is an Au metal.
[0035] See also Figures 2 to 9 As shown, the preparation method of the metal thin layer structure for surface bonding provided by the present invention is further described in detail below:
[0036] Step 1: A first metal layer 1 with a thickness of 100 nm is prepared on the surface of the capacitor medium 8 by using a WTi mixed metal target and a magnetron sputtering process, wherein the mass ratio of W to Ti in the WTi mixed metal target is 3:7. The first metal layer 1 can serve as a seed layer to increase the adhesion between the capacitor medium (8) and the metal, such as Figure 2 shown.
[0037] Step 2: Using Au metal target and magnetron sputtering process to prepare a second metal layer 2 with a thickness of 95nm, wherein the purity of Au metal target is higher than 99.999%, and the second metal layer 2 is used as a seed layer for electroplating the third metal layer 3 to enhance the adhesion. Figure 3 shown.
[0038] Step 3: Use a photolithography process to coat and cure the photoresist 7 in the area where the third metal layer 3 is not required, and expose the area where the third metal layer 3 is required. Figure 4 shown.
[0039] Step 4: Use Ni metal target material and prepare a third metal layer 3 with a thickness of 800nm through electroplating process. The third metal layer 3 can improve the bonding strength of the overall structure, such as Figure 5 shown.
[0040] Step 5: Use a WTi mixed metal target and prepare a fourth metal layer 4 with a thickness of 100 nm by magnetron sputtering process, wherein the mass ratio of W to Ti in the WTi mixed metal target is 3:7, such as Figure 6 shown.
[0041] Step 6: Using Au metal target and using magnetron sputtering process to prepare a fifth metal layer 5 with a thickness of 95 nm, wherein the purity of the Au metal target is higher than 99.999%, such as Figure 7shown.
[0042] Step 7: Use Au metal target and prepare a sixth metal layer 6 with a thickness of 1.5 μm through photoplating process. The sixth metal layer 6 is used as a gold wire bonding layer. In addition to being used for gold wire bonding, it also releases the stress during the bonding process. Figure 8 shown.
[0043] Step 8: The photoresist 7 is stripped by wet solvent stripping, and the third metal layer 3, the fourth metal layer 4, the fifth metal layer 5 and the sixth metal layer 6 on the photoresist 7 are stripped accordingly. Fig. 9 shown.
[0044] Step 9: Remove the excess second metal layer 2 below the area without the third metal layer 3 by a wet process. The wet solution used is a mixture of potassium cyanide: 647 gold removal concentrate: water with a volume ratio of 1:5:200. The etching time is 90 seconds. Fig. 9 shown.
[0045] Step 10: Remove the excess first metal layer 1 below the area without the third metal layer 3 by a wet process. The wet solution used is hydrogen peroxide. The hydrogen peroxide temperature is 60° C., the concentration is 26%, and the etching time is 110 seconds. Fig. 9 shown.
[0046] The bonding strength of the prepared metal thin layer was tested and compared with a metal thin layer sheet in the prior art: the bonding strength of 22 points on the metal thin layer prepared by the present invention was measured respectively, and the results were all greater than 60 grams, which met the characteristics of high bonding tensile strength; while the bonding strength of 22 points at the same position of the metal thin layer sheet of the prior art for comparison was between 12.5 grams and 19.9 grams, which is quite different from the bonding strength index of the metal thin layer structure prepared by the present invention.
Claims
1. A metal thin layer structure for surface bonding, It is characterized in that The invention comprises a first metal layer (1), a second metal layer (2) arranged on the first metal layer (1), a third metal layer (3) arranged on the second metal layer (2), a fourth metal layer (4) arranged on the third metal layer (3), a fifth metal layer (5) arranged on the fourth metal layer (4), and a sixth metal layer (6) arranged on the fifth metal layer (5); the first metal layer (1) is a WTi mixed metal, the second metal layer (2) is an Au metal, the third metal layer (3) is a Ni metal, the fourth metal layer (4) is a WTi mixed metal, the fifth metal layer (5) is an Au metal, and the sixth metal layer (6) is an Au metal.
2. A method for preparing a metal thin layer structure for surface bonding as claimed in claim 1, It is characterized in that The following steps are involved: S1. The first metal layer (1) is prepared by a WTi mixed metal target and a magnetron sputtering process; S2. The second metal layer (2) is prepared by using an Au metal target and a magnetron sputtering process; S3. The photoresist (7) is coated and cured in the region where the third metal layer (3) is not required to be prepared by a photolithography process, and the region where the third metal layer (3) is required to be prepared is exposed; S4. The third metal layer (3) is prepared by using a Ni metal target and an electroplating process; S5. The fourth metal layer (4) is prepared by a WTi mixed metal target and a magnetron sputtering process; S6. The fifth metal layer (5) is prepared by using an Au metal target and a magnetron sputtering process; S7. The sixth metal layer (6) is prepared by using an Au metal target and a photoplating process; S8. Stripping the photoresist (7); S9. Remove the redundant second metal layer (2) and first metal layer (1) below the area without the third metal layer (3).
3. The method for preparing the metal thin layer structure for surface bonding according to claim 2, It is characterized in that The mass ratio of W metal to Ti metal in the WTi mixed metal target is 2:8 to 5:
5.
4. The method for preparing the metal thin layer structure for surface bonding according to claim 2, It is characterized in that In S1, a capacitor medium (8) is prepared, and a first metal layer (1) is formed on the surface of the capacitor medium (8) by a magnetron sputtering process.
5. The method for preparing the metal thin layer structure for surface bonding according to claim 2, It is characterized in that The first metal layer (1) serves as a seed layer, and the second metal layer (2) serves as a seed layer for electroplating the third metal layer (3).
6. The method for preparing a metal thin layer structure for surface bonding according to claim 2, It is characterized in that In S8, while removing the photoresist (7), the third metal layer (3), the fourth metal layer (4), the fifth metal layer (5), and the sixth metal layer (6) on the photoresist (7) are peeled off along with the photoresist (7).
7. The method for preparing a metal thin layer structure for surface bonding according to claim 2, It is characterized in that The sixth metal layer (6) serves as a gold wire bonding layer.
8. The method for preparing a metal thin layer structure for surface bonding according to claim 2, It is characterized in that The thickness of the first metal layer (1) is 40 to 150 nm, the thickness of the second metal layer (2) is 20 to 160 nm, the thickness of the third metal layer (3) is 350 to 1300 nm, the thickness of the fourth metal layer (4) is 40 to 150 nm, the thickness of the fifth metal layer (5) is 20 to 160 nm, and the thickness of the sixth metal layer (6) is 1.1 to 5 μm.
9. The method for preparing a metal thin layer structure for surface bonding according to claim 2, It is characterized in that In S9, when a wet process is used to remove the excess second metal layer (2) below the area without the third metal layer (3), the wet solution used is a mixture of potassium cyanide: 647 gold removal concentrate: water in a volume ratio of 1:5:200; when a wet process is used to remove the excess first metal layer (1) below the area without the third metal layer (3), the wet solution used is hydrogen peroxide, the temperature is 60°C, and the concentration is 26%.
10. The method for preparing a metal thin layer structure for surface bonding according to claim 2, It is characterized in that The purity of the Au metal target material is higher than 99.999%.
Citation Information
Patent Citations
GaN-based HEMT gold-free ohmic contact electrode and thermal nitridation forming method thereof
CN110556419A
GaN-based HEMT gold-free ohmic contact electrode based on Ti / Ti-Al / Cu-W and preparation method of GaN-based HEMT gold-free ohmic contact electrode
CN112670337A
Conductive film, pole piece, electrochemical device, coating equipment and coating method
CN116844759A
Reduced reflectance display devices containing a thin-layer metal-organic mixed layer (MOML)
CN1866575A
Contacts for Semiconductor Devices and Methods of Forming Thereof
US20160005647A1