Nano-diamond coating and preparation method thereof
By using hot wire chemical vapor deposition method on cemented carbide tools, nanodiamond coatings are deposited using hydrogen, methane and nitrogen, the problem of insufficient hardness of nanodiamond coatings is solved, the hardness and processing quality of the tool are improved, and the tool is extended Lifespan, especially in finishing fiber composites and hot-bending graphite molds.
Patent Information
- Application Number
- CN202411176995.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing nanodiamond coatings have insufficient hardness, resulting in accelerated tool wear and reduced processing quality, especially when finishing fiber composite materials and hot-bending graphite molds, there are differences in cutter defects and roughness.
The nanodiamond coating is deposited on the microdiamond coating by hot wire chemical vapor deposition method, using hydrogen, methane and nitrogen as the deposition gas to control the pressure and flow ratio of the deposition gas, and the matrix temperature is between 800℃ and 950℃ to form a high hardness The nanodiamond coating has a diamond phase content of more than 60%, and a hardness of more than 80GPa.
It improves the hardness of the nanodiamond coating, extends the tool life, improves processing quality, especially in finished fiber composites and hot-bending graphite molds, and reduces tool wear and roughness differences in workpieces after processing.
Smart Images

Figure CN119040845A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond coatings, and relates to a nano-diamond coating and a preparation method thereof, and specifically relates to a nano-diamond coating for a cemented carbide tool and a preparation method thereof. Background Art
[0002] Hot wire chemical vapor deposition (HFCVD) technology has the advantages of low cost, simple equipment, stable process, and suitability for complex shapes and large-area deposition. It is currently the most commonly used method for preparing diamond-coated carbide tools. Chemical vapor deposition (CVD) diamond coating has excellent properties such as high hardness, high wear resistance, and low friction coefficient close to natural diamonds. Depositing on the surface of carbide tools can greatly increase the service life of the tools and improve the processing quality of the workpiece. In order to adapt to the working conditions under different environments, researchers have developed micron diamond coatings and nano diamond coatings.
[0003] Micron diamond coating has a columnar crystal structure, with a grain size of 1-5μm, high crystallinity, and less impurities in the diamond coating. It has a hardness and elastic modulus close to that of natural diamond. As a protective layer for cemented carbide tools, it makes cemented carbide tools have excellent wear resistance, can reduce the wear rate of tools, and increase the life of tools. However, its rough surface is easy to cause fiber composite material delamination and graphite hot bending mold knife mark defects when used in fiber composite finishing and graphite hot bending mold super finishing.
[0004] Nano-diamond coating has a smooth surface. When used as a coating for cutting tools, it can reduce the surface roughness of the workpiece and improve the processing quality. Nano-diamond coatings for cutting tools are generally deposited using HFCVD. The conventional deposition process is: 1) In a hydrogen and methane deposition system, a large amount of argon is added, the argon content reaches more than 60%, and the deposition gas pressure is less than 1.6kPa to form nanocrystals. 2) In a hydrogen and methane deposition system, a large amount of methane gas is introduced, the methane concentration reaches more than 4%, and the deposition gas pressure is less than 1.2kPa to form nanocrystals. However, the increase in carbon source concentration causes the nano-diamond coating to produce amorphous carbon and graphite phases during the formation process, reducing the content and hardness of the diamond phase in the diamond coating. The diamond phase content in the diamond coating deposited by this method is usually less than 60%, and its hardness value is generally 50-75GPa. In practical applications, the presence of graphite phase and amorphous carbon phase and the reduction in hardness of the nano-diamond coating will lead to accelerated tool wear and changes in the angle of the tool cutting edge. The processed 5G mobile phone graphite hot bending mold will have a significant difference in roughness between the front and rear processing areas, and even obvious color difference, resulting in the scrapping of the workpiece. Therefore, it is necessary to develop high-hardness nano-diamond coatings to increase the life of the tool. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, and in particular to address the technical problem of insufficient hardness of nano-diamond coatings, to provide a nano-diamond coating with high hardness and a preparation method thereof. The nano-diamond coating prepared by the present invention has the characteristics of high diamond phase content and high hardness in the Raman spectrum, and can improve the tool life of coated tools in fine processing of fiber composite materials and hot-bending graphite molds.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions.
[0007] A nano-diamond coating has an average grain size of less than 80nm, a diamond phase content of more than 60% in the Raman spectrum of the nano-diamond coating, and a thickness of 3μm to 30μm.
[0008] The above-mentioned nano-diamond coating, preferably, has an average grain size of less than 50 nm.
[0009] Preferably, the nano-diamond coating has a diamond phase content greater than 65% in its Raman spectrum.
[0010] The nano-diamond coating mentioned above, preferably, has a hardness greater than 80 GPa.
[0011] More preferably, the nano-diamond coating has a hardness greater than 85 GPa.
[0012] As a general technical concept, the present invention also provides a method for preparing the above-mentioned nano-diamond coating, comprising the following steps:
[0013] (1) Nucleation: Depositing a layer of micron diamond coating on the pretreated carbide tool substrate;
[0014] (2) Depositing a nano-diamond coating: A hot wire chemical vapor deposition method is used to deposit a nano-diamond coating on the micron diamond coating, wherein hydrogen, methane and nitrogen are used as deposition gases, the flow ratio of methane to hydrogen is 1:30-100, the flow ratio of nitrogen to methane is 1:0.1-3, the deposition gas pressure is 3 kPa-8.5 kPa, and the substrate temperature is 800°C-950°C. After deposition, a nano-diamond coating is obtained.
[0015] In the above-mentioned method for preparing the nanodiamond coating, preferably, in step (2), the flow ratio of methane to hydrogen is 1:30-70, the flow ratio of nitrogen to methane is 1:0.3-2.5, the deposition gas pressure is 3kPa-7kPa, and the substrate temperature is 850°C-950°C.
[0016] The above-mentioned method for preparing the nano-diamond coating, preferably, in step (1), the micron diamond coating is deposited by hot wire chemical vapor deposition, hydrogen and methane are used as deposition gases, the flow ratio of methane to hydrogen is 1:30-80, the deposition gas pressure is 1kPa-2kPa, the substrate temperature is 750°C-950°C, and the thickness of the micron diamond coating is 0.1μm-2μm.
[0017] The above-mentioned method for preparing the nano-diamond coating is more preferably, in step (1), the flow ratio of methane to hydrogen is 1:40-60, the deposition gas pressure of the deposition chamber is 1.2kPa-1.6kPa, the substrate temperature is 800°C-900°C, and the thickness of the micron diamond coating is 0.5μm-1μm.
[0018] In the above-mentioned method for preparing the nano-diamond coating, preferably, in step (1), the cemented carbide used in the cemented carbide tool substrate is a cemented carbide with a cobalt content of no more than 6wt%, and the pretreatment includes WC phase pretreatment, Co phase pretreatment and crystal planting treatment;
[0019] The WC phase pretreatment process is to place the cemented carbide tool substrate in a mixed aqueous solution of potassium ferrocyanide and sodium hydroxide for ultrasonic treatment, and then spray and air-dry; wherein the mass ratio of potassium ferrocyanide, sodium hydroxide, and water in the mixed aqueous solution of potassium ferrocyanide and sodium hydroxide is 1:1:10-20, and the ultrasonic treatment time is 10min-30min;
[0020] The Co phase pretreatment process is to immerse the cemented carbide tool substrate after the WC phase pretreatment in a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the mass ratio of sulfuric acid, hydrogen peroxide and water is 1:1:100-200, the mass concentration of sulfuric acid is 98%, the mass concentration of hydrogen peroxide is 30%, and the immersion time is 1 min-5 min;
[0021] The process of the crystal planting treatment is to add the cemented carbide tool substrate after the Co phase pretreatment into the diamond micropowder suspension for ultrasonic treatment, the diamond micropowder in the diamond micropowder suspension has a grain size of 0.05μm to 3μm, and the ultrasonic treatment time is 15min to 60min.
[0022] In the present invention, the diamond phase content Q in the diamond coating is defined as: D / I T , where I D Refers to the intensity value of the diamond characteristic peak in the Raman spectrum of the diamond coating, I T It refers to the sum of the intensities of all peaks in the Raman spectrum. The intensities of different peaks are calculated based on the peak separation and Gaussian fitting of the Raman spectrum. The sensitivity of non-diamond phase in Raman characterization is much higher than that of diamond phase, and the sensitivity of graphite phase is about 50-75 times that of diamond. Therefore, I T =I D +(I1+……I n ) / 50.
[0023] In the present invention, the average grain size of the diamond coating is obtained by measuring the half-width of the diffraction peak of the diamond coating (111) from an X-ray diffraction spectrum, and the average grain size of the diamond coating is calculated using the Scherrer formula.
[0024] D=Kλ / Bcosθ
[0025] Wherein, D is the grain size of the test sample in the direction of the diffraction crystal plane, K is the Scherrer constant, K=0.89, λ is the X-ray wavelength, which is 0.154 nm, B is the half-height width of the diffraction peak of the measured sample, and θ is the Bragg diffraction angle, in degrees.
[0026] In practical applications, the thickness of the nano-diamond coating on the nano-diamond coated carbide CNC blades can reach 3-25μm, and the thickness of the nano-diamond coating on the nano-diamond coated carbide integral tool is 3-15μm. The CNC blade has a relatively blunt edge and can be used for rough machining, so the coating is relatively thick. In most cases, the integral tool is used for fine machining, and the coating thickness is relatively thin.
[0027] Compared with the prior art, the advantages of the present invention are:
[0028] (1) The nano-diamond coating of the present invention is prepared by hot wire chemical vapor deposition, and nitrogen is added to the methane and hydrogen deposition system. During the growth of the diamond coating, a high-hardness nano-diamond coating is formed. The hardness of the nano-diamond coating deposited by the present invention is higher than the hardness of the nano-diamond coating deposited by the CH4-H2-(Ar) deposition system. Usually, the hydrogen-methane deposition system obtains the nano-diamond coating by reducing the pressure of the deposition gas chamber or greatly increasing the methane concentration, forming a large number of carbon-containing groups (CHx, Cx) in the chamber, and forming a nano-coating through secondary nucleation. During the reaction process, a large number of carbon-containing groups cannot react completely with hydrogen, resulting in excessive non-diamond phases in the coating. The deposition method of the present invention is formed by introducing a small amount of nitrogen on the basis of the micron diamond coating deposition process. The nitrogen is decomposed to form N atoms, which accelerates the hydrogen extraction step in the diamond coating formation process, thereby accelerating the reaction rate and forming nanocrystals. The formed nanocrystals have a high diamond phase content and higher hardness. The hardness value is greater than 80GPa, which can extend the tool life, especially the tool life of the coated tool in the fine processing of fiber composite materials and hot bending graphite molds, and improve the quality of the processed workpiece.
[0029] (2) The preparation method of the present invention is simple and effective, and is conducive to industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a surface morphology of the nano-diamond coating deposited in Example 1 of the present invention.
[0031] Figure 2 This is the Raman spectrum of the nano-diamond coating deposited in Example 1 of the present invention.
[0032] Figure 3 This is the X-ray diffraction pattern of the nano-diamond coating deposited in Example 1 of the present invention.
[0033] Figure 4 This is a hardness test diagram of the nano-diamond coating deposited in Example 1 of the present invention.
[0034] Figure 5 This is the Raman spectrum of the nano-diamond coating deposited in Example 2 of the present invention.
[0035] Figure 6 This is a hardness test diagram of the nano-diamond coating deposited in Example 2 of the present invention.
[0036] Figure 7 This is the surface morphology of the deposited coating in Comparative Example 2. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.
[0038] Example 1
[0039] The nano-diamond coating of the present invention has an average grain size of 15nm, a diamond phase content of 77.4% in the Raman spectrum of the nano-diamond coating, a thickness of 15.8μm, and a hardness of 90.5GPa.
[0040] A method for preparing a nano-diamond coating of the present invention comprises the following steps:
[0041] (1) Matrix pretreatment: The cemented carbide tool matrix used is a cemented carbide ps strip with WC-Co 6wt% and a specification of 6mm×5mm×21mm. First, the cemented carbide tool matrix is pretreated, and the pretreatment includes WC phase pretreatment, Co phase pretreatment and crystal planting treatment. The specific process is: the cemented carbide tool matrix is ultrasonically treated in a potassium ferrocyanide and sodium hydroxide solution for 30 minutes, and the mass ratio of potassium ferrocyanide, sodium hydroxide and water in the mixed aqueous solution of potassium ferrocyanide and sodium hydroxide is 1:1:10. After spraying and air-drying, it is placed in a mixed aqueous solution of sulfuric acid and hydrogen peroxide for 90 seconds. The mass ratio of sulfuric acid, hydrogen peroxide and water in the mixed aqueous solution of sulfuric acid and hydrogen peroxide is 1:1:100, the mass concentration of sulfuric acid is 98%, and the mass concentration of hydrogen peroxide is 30%. Then, it is placed in a 3μm diamond micropowder suspension for ultrasonic treatment for 20 minutes. The obtained ps strip is washed with pure water and air-dried to obtain a pretreated cemented carbide tool matrix.
[0042] (2) Nucleation: The pretreated carbide tool substrate was placed in the diamond coating chamber and deposited by hot wire chemical vapor deposition (HFCVD). Hydrogen and methane were introduced. The methane gas flow rate was 32 sccm, the hydrogen flow rate was 1600 sccm, the deposition gas pressure in the deposition chamber was 1.5 kPa, the substrate temperature was 900 °C, and the deposition time was 40 min. A micron diamond coating with a thickness of 800 nm was obtained.
[0043] (3) Nanodiamond coating deposition: After the nucleation process is completed, the flow rates of methane and hydrogen are kept unchanged, the substrate temperature remains unchanged, and nitrogen is introduced. The nitrogen flow rate is 16 sccm, the deposition gas pressure in the deposition chamber is 3.3 kPa, and the deposition time is 10 h. A nanodiamond coating with a thickness of 15.8 μm is obtained.
[0044] Figure 1 This is the surface morphology of the nano-diamond coating prepared in this example. The surface of the diamond coating is flat and the coating thickness is 15.8 μm. Figure 2 This is the Raman spectrum of the nano-diamond coating prepared in this embodiment. After analysis, it can be seen that the residual stress of the nano-diamond coating is -1.03 GPa, and the diamond phase content is 77.4%. Figure 3 The X-ray diffraction spectrum of the nano-diamond coating prepared in this example shows that the half-height width of the (111) diffraction peak is 0.565, and the average grain size of the coating is calculated to be 15 nm. Figure 4 The nanohardness of the nanodiamond coating of this embodiment is measured, and the hardness value is 90.5GPa. At the same time, the prepared nanodiamond coating cemented carbide is tested for indentation bonding performance in accordance with GB / T36591-2018 "Metallographic Detection Method for Coating of Cemented Carbide Products", and the peeling grade is P1.
[0045] Example 2
[0046] The invention discloses a nano-diamond coating, wherein the average grain size of the nano-diamond coating is 13nm, the diamond phase content in the Raman spectrum of the nano-diamond coating is 69%, the thickness of the nano-diamond coating is 11μm, and the hardness is 85GPa.
[0047] A method for preparing a nano-diamond coating of the present invention comprises the following steps:
[0048] (1) Substrate pretreatment: The substrate of the cemented carbide tool used is a cemented carbide furnace control rod of WC-Co6wt% and a specification of D8mm×75mm. The furnace control rod has two parallel sides, and the size of the parallel sides is 6mm×75mm. At the same time, a four-edge milling cutter of D6mm×70mm is placed in the furnace control rod for pretreatment and coating. The pretreatment process is the same as that of Example 1.
[0049] (2) Nucleation: The pretreated carbide tool substrate was placed in the diamond coating chamber and deposited by HFCVD method. Hydrogen and methane were introduced. The substrate temperature was 930°C, the methane gas flow rate was 32 sccm, the hydrogen flow rate was 1600 sccm, the gas pressure in the deposition chamber was 1.5 kPa, and the deposition time was 0.5 h. A micron diamond coating with a thickness of 0.8 μm was obtained.
[0050] (3) Nanodiamond coating deposition: After the nucleation process is completed, the flow rates of methane and hydrogen are kept unchanged, the substrate temperature is 900°C, nitrogen is introduced, the nitrogen flow rate is 48 sccm, the gas pressure in the deposition chamber is 4 kPa, and the deposition time is 10 h to obtain a nanodiamond coating with a thickness of 11 μm.
[0051] Figure 5 The Raman spectrum of the nano-diamond coating prepared in this example shows, after peak separation and Gaussian fitting, that the residual stress of the diamond coating is -1.19 GPa and the diamond phase content is 69%. Figure 6 The nanohardness of the nanodiamond coating of this embodiment is measured, and the hardness value is 85GPa. After the diamond coating indentation bonding performance test, the hard peeling grade of the prepared nanodiamond coating is P1. The cutting performance test of the cemented carbide tool containing the nanodiamond coating prepared in this embodiment, the cutting material is T700 carbon fiber reinforced resin-based composite material, and the cutting parameters are V=150m / min, ap=2mm, ae=0.1mm, fz=0.05mm / r. The wear of the tool back face is observed every hour. The tool back face wear value of this embodiment is 0.089mm after 4 hours of processing, while the tool back face wear value of the conventional nanodiamond coating tool has reached 0.09mm after 2 hours of processing. The tool life of this embodiment is about twice that of the conventional nano coating.
[0052] Comparative Example 1
[0053] The same cemented carbide PS strip was used as in Example 1, and the pretreatment and nucleation processes were the same. The gas added in the coating process was changed from nitrogen to argon, and the deposition parameters remained unchanged. The specific parameters were:
[0054] The methane gas flow rate is 32 sccm, the hydrogen gas flow rate is 1600 sccm, the deposition chamber gas pressure is 3.3 kPa, the substrate temperature is 900°C, the argon gas flow rate is 16 sccm, and the deposition time is 10 hours. The obtained coating is a micron coating with a coating grain size of 3-7 μm. The preparation of nano coating failed under this deposition condition.
[0055] Comparative Example 2
[0056] The same cemented carbide PS strip was used as in Example 1, and the pretreatment and nucleation processes were the same. The content of nitrogen added in the coating process was changed. The specific parameters were:
[0057] The methane gas flow rate is 32sccm, the hydrogen flow rate is 1600sccm, the deposition chamber gas pressure is 3.3kPa, the substrate temperature is 900℃, the nitrogen flow rate is 10sccm, and the deposition time is 10h. The obtained coating is mainly micron and submicron crystals, with a small amount of nano-crystals. The grain size of the coating is 0.3-6μm. Figure 7 As shown in Figure 4, the nanocoating failed to be prepared under this deposition condition.
[0058] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A nano-diamond coating, characterized in that: The average grain size of the nano-diamond coating is below 80nm, the diamond phase content in the Raman spectrum of the nano-diamond coating is greater than 60%, and the thickness of the nano-diamond coating is 3μm to 30μm.
2. The nano-diamond coating according to claim 1, characterized in that: The average grain size of the nano-diamond coating is below 50 nm.
3. The nano-diamond coating according to claim 1, characterized in that: The diamond phase content in the Raman spectrum of the nano-diamond coating is greater than 65%.
4. The nano-diamond coating according to any one of claims 1 to 3, characterized in that: The hardness of the nano-diamond coating is greater than 80 GPa.
5. The nano-diamond coating according to claim 4, characterized in that: The hardness of the nano-diamond coating is greater than 85 GPa.
6. A method for preparing a nano-diamond coating as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Nucleation: Depositing a layer of micron diamond coating on the pretreated carbide tool substrate; (2) Depositing a nano-diamond coating: A hot wire chemical vapor deposition method is used to deposit a nano-diamond coating on the micron diamond coating, wherein hydrogen, methane and nitrogen are used as deposition gases, the flow ratio of methane to hydrogen is 1:30-100, the flow ratio of nitrogen to methane is 1:0.1-3, the deposition gas pressure is 3 kPa-8.5 kPa, and the substrate temperature is 800°C-950°C. After deposition, a nano-diamond coating is obtained.
7. The method for preparing the nano-diamond coating according to claim 6, characterized in that: In step (2), the flow ratio of methane to hydrogen is 1:30-70, the flow ratio of nitrogen to methane is 1:0.3-2.5, the deposition gas pressure is 3 kPa-7 kPa, and the substrate temperature is 850°C-950°C.
8. The method for preparing the nano-diamond coating according to claim 6 or 7, characterized in that: In step (1), the micron diamond coating is deposited by hot wire chemical vapor deposition, with hydrogen and methane as deposition gases, the flow ratio of methane to hydrogen is 1:30-80, the deposition gas pressure is 1 kPa-2 kPa, the substrate temperature is 750°C-950°C, and the thickness of the micron diamond coating is 0.1 μm-2 μm.
9. The method for preparing the nano-diamond coating according to claim 8, characterized in that: In step (1), the flow ratio of methane to hydrogen is 1:40-60, the deposition gas pressure of the deposition chamber is 1.2 kPa-1.6 kPa, the substrate temperature is 800° C.-900° C., and the thickness of the micron diamond coating is 0.5 μm-1 μm.
10. The method for preparing the nano-diamond coating according to claim 6 or 7, characterized in that: In step (1), the cemented carbide used in the cemented carbide tool substrate is a cemented carbide with a cobalt content of no more than 6wt%, and the pretreatment includes WC phase pretreatment, Co phase pretreatment and crystal planting treatment; The WC phase pretreatment process is to place the cemented carbide tool substrate in a mixed aqueous solution of potassium ferrocyanide and sodium hydroxide for ultrasonic treatment, and then spray and air-dry; wherein the mass ratio of potassium ferrocyanide, sodium hydroxide, and water in the mixed aqueous solution of potassium ferrocyanide and sodium hydroxide is 1:1:10-20, and the ultrasonic treatment time is 10min-30min; The Co phase pretreatment process is to immerse the cemented carbide tool substrate after the WC phase pretreatment in a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the mass ratio of sulfuric acid, hydrogen peroxide and water is 1:1:100-200, the mass concentration of sulfuric acid is 98%, the mass concentration of hydrogen peroxide is 30%, and the immersion time is 1 min-5 min; The process of the crystal planting treatment is to add the cemented carbide tool substrate after the Co phase pretreatment into the diamond micropowder suspension for ultrasonic treatment, the diamond micropowder in the diamond micropowder suspension has a grain size of 0.05μm to 3μm, and the ultrasonic treatment time is 15min to 60min.