Method for constructing antifriction lubricating interface structure on surface of titanium alloy

By using plasma electrolytic oxidation technology on the surface of titanium alloy, and combining with Ti3C2 nanocoating, a composite interface structure is formed, which solves the problem of poor tribological properties of titanium alloy, and achieves wear resistance and self-lubricating effects. It is suitable for a variety of purposes Application field.

CN119040889APending Publication Date: 2024-11-29XIAN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410838471.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Titanium alloys have problems with poor tribological properties and unstable mechanical properties in aerospace, precision manufacturing and biomedical applications. Traditional surface treatment methods such as anodization, thermal spraying and chemical vapor deposition have severe pollution, limited reinforcement effects and compatible interfaces. Poor sex problem.

Method used

The ceramic coating is grown in situ on the surface of titanium alloy by plasma electrolytic oxidation technology, and combined with the Ti3C2 nanocoating to form a composite interface structure. The porous structure of the PEO coating and the low friction characteristics of the Ti3C2 coating are used to jointly exert their respective advantages. Form an interface that is wear-resistant and self-lubricating.

Benefits of technology

It significantly reduces the coefficient of friction, improves wear resistance and corrosion resistance, and reduces wear. It is suitable for mechanical manufacturing, automotive body hardening, marine manufacturing, aerospace wear-resistant components and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040889A_ABST
    Figure CN119040889A_ABST
Patent Text Reader

Abstract

The invention discloses a method for constructing an antifriction lubricating interface structure on the surface of a titanium alloy. The method comprises the steps that 1, the surface of a titanium alloy grinding disc is pretreated; 2, sodium silicate is prepared, sodium hexametaphosphate, sodium bicarbonate, ammonium vanadate and potassium fluoride are placed in water and stirred to be completely dissolved, and then an electrolyte is obtained; 3, the TC6 millstone obtained in the step 1 is placed in the electrolyte obtained in the step 2, plasma electrolytic oxidation is conducted in a constant-current control mode, and the millstone with a PEO coating on the surface is obtained; step 4, etching Ti3AlC2 in hydrofluoric acid, then repeatedly cleaning the Ti3AlC2 in plasma water, dispersing the purified Ti3C2 nanoparticles in a propyl alcohol solution, and preparing a dispersion liquid after ultrasonic dispersion; and step 5, coating the Ti3C2 nano-particles prepared in the step 4 on a horizontally placed titanium alloy millstone to obtain the titanium alloy millstone PEO-Ti3C2 of which the surface is provided with a Ti3C2 coating and a PEO coating. Plasma electrolytic oxidation is combined with a two-dimensional material nano coating, so that a friction interface structure is customized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy surface treatment and relates to a method for constructing a friction-reducing and lubricating interface structure on the surface of a titanium alloy. Background Art

[0002] Although titanium alloys have great potential in aerospace, precision manufacturing and biomedical applications, their poor tribological properties and unstable mechanical characteristics pose challenges to their wider application. Traditional surface braiding and solid lubricants can provide protection for the matrix, but often cause defects due to the different morphologies of the reinforcement and matrix and the structural incompatibility between the materials.

[0003] Inspired by the armadillo bone-skin-hair structure, we propose a self-lubricating, wear-resistant interface structure by in-situ growing a ceramic coating on a titanium alloy substrate followed by deposition of a Ti3C2Tx nanocoating. This approach reduces the coefficient of friction from 0.89 to 0.41, which is equivalent to that of a polished to mirror-finish substrate (0.4), greatly reducing wear and providing excellent substrate protection. During the friction process, the microporous interface structure absorbs 2D MXenes and rapidly transfers lubricants to the wear interface through grinding, while continuously adding new lubricants during the cycle. In addition, the continuous decomposition and recombination of the MXene coating forms a strong tribofilm that resists oxidation and plastic deformation of the subsurface layer, thereby greatly improving the wear resistance. The tribointerface structure is customized by combining plasma electrolytic oxidation with 2D material nanocoating through a simple and effective strategy, which is consistent with the unique biological protection mechanism. These findings are crucial for future PEO technology and the development of new materials aimed at optimizing tribological properties. They are essential for advancing titanium alloys toward a wider range of applications.

[0004] For centuries, scholars around the world have developed a series of surface strengthening technologies to improve the tribological properties of titanium alloys, including anodizing, thermal spraying, laser surface texturing, and chemical vapor deposition. However, these methods all have various defects, such as severe pollution, limited enhancement effect, and poor interface compatibility, which makes their widespread application challenging. The unique protection mechanism of organisms such as armadillos provides valuable inspiration for the development of friction-reducing and wear-resistant structures. Specifically, designing a protective structure similar to the bone-skin interface of these animals to protect the titanium alloy substrate is a promising approach. Advances in PEO technology and the development of two-dimensional materials (such as MXenes) provide a feasible strategy to address these challenges.

[0005] In view of the effectiveness and limitations of the above methods, we draw inspiration from the armadillo skin structure and use PEO technology to grow in-situ ceramic coatings on titanium alloys with excellent adhesion and mechanical properties. In addition, by making the PEO coating hydrophilic and easy to combine with lubricants, and combining its porous structure and wear-resistant properties with the low-friction lubricating properties of MXene coatings, we designed a composite strategy that synergistically exerts the respective advantages of PEO and MXene coatings, heralding a paradigm shift in the tribological properties of titanium alloys. In other words, by taking advantage of the micropore and microcrack structure to capture and store lubricating particles, as well as the obvious friction anisotropy, we cleverly transformed the typical structure of PEO coatings into a coating that can generate friction resistance on the surface of titanium alloys. In view of the effectiveness and limitations of the above methods, we draw inspiration from the armadillo skin structure and use PEO technology to grow in-situ ceramic coatings on titanium alloys with excellent adhesion and mechanical properties. Summary of the invention

[0006] The purpose of the present invention is to provide a method for constructing a friction-reducing and lubricating interface structure on the surface of a titanium alloy, which adopts plasma electrolytic oxidation technology and a Ti3C2 coating to customize the friction-reducing and lubricating interface structure, thereby solving the problems of large friction coefficient and unstable friction-reducing and lubricating effect of the existing coating prepared by plasma electrolytic oxidation.

[0007] The technical solution adopted by the present invention is a method for constructing a friction-reducing and lubricating interface structure on the surface of a titanium alloy, including in-situ growth of a hard ceramic coating by plasma electrolytic oxidation and coating of a two-dimensional material Ti3C2 with low shear force by drop casting. The method is specifically implemented in the following steps:

[0008] Step 1, pre-treating the surface of the titanium alloy grinding disc;

[0009] Step 2, sodium silicate, sodium hexametaphosphate, sodium bicarbonate, ammonium vanadate and potassium fluoride are placed in water and stirred until all dissolved to obtain an electrolyte;

[0010] Step 3, placing the TC6 grinding disc obtained in step 1 in the electrolyte obtained in step 2, and performing plasma electrolytic oxidation in a constant current control mode to obtain a grinding disc with a PEO coating on the surface;

[0011] Step 4, etching Ti3AlC2 in hydrofluoric acid, then repeatedly washing with plasma water, dispersing the purified Ti3C2 nanoparticles in a propanol solution, and preparing a dispersion after ultrasonic dispersion;

[0012] Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface;

[0013] In step 1, the surface of the titanium alloy grinding disc is pretreated, including polishing the surface of the titanium alloy grinding disc with silicon carbide sandpaper and flannel. Specifically, the surface of the titanium alloy grinding disc is first polished with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then polished with 2000 mesh flannel. The sandpaper is silicon carbide sandpaper, so that the surface is free of foreign matter and smooth.

[0014] In the electrolyte prepared in step 2, the concentration of sodium hexametaphosphate is 12-18 g / L, the concentration of sodium hydroxide is 2.5-3.5 g / L, the concentration of sodium silicate is 10-15 g / L, the concentration of ammonium metavanadate is 2.5-4.5 g / L, and the concentration of potassium fluoride is 0.5-1.0 g / L. The stirring speed is 800-1100 r / min, and the stirring time is 25 min-30 min.

[0015] In step 3, the plasma electrolytic oxidation is carried out in a constant current control mode, and the positive current and negative current are set to 1.3-1.7A and 0.1-0.5A / dm respectively. 2 The pulse frequency is set to 400Hz~600Hz, the positive and negative duty cycles are both 12%~22%, and the response time is set to 13min~16min.

[0016] In step 4, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

[0017] The titanium alloy grinding disc is made of TC6 alloy.

[0018] The beneficial effects of the present invention are as follows:

[0019] (1) The present invention firstly utilizes plasma electrolytic oxidation technology to in-situ grow a ceramic coating with excellent adhesion and mechanical properties on titanium alloy. In addition, by making the PEO coating hydrophilic, it is easy to combine with lubricants, and its porous structure and wear resistance are combined with the low friction lubrication properties of the Ti3C2 coating;

[0020] (2) We devised a composite strategy that synergistically exploits the respective advantages of PEO and Ti3C2 coatings, heralding a paradigm shift in the tribological properties of titanium alloys. In other words, by taking advantage of the micropore and microcrack structures to capture and store lubricating particles, as well as the pronounced friction anisotropy, we cleverly transformed the typical structure of PEO coatings into a coating that can generate friction resistance on titanium alloy surfaces.

[0021] (3) The present invention adopts a constant current control mode after optimizing electrical parameters for plasma electrolytic oxidation. This method has the advantages of low energy consumption and stable discharge effect. In addition, the phosphate-silicate electrolyte system used is a low-cost electrolyte and is easy to obtain.

[0022] (4) The present invention customizes a bone-skin type composite interface structure on the surface of titanium alloy through plasma electrolytic oxidation technology and two-dimensional material Ti3C2. The structure is dense and uniform, with a combination of soft and hard surfaces. Compared with the titanium alloy matrix, the wear rate is reduced by more than 10 times. In addition, the coating has good surface properties and has both wear resistance and corrosion resistance. It can be used in machinery manufacturing, automobile body hardening, shipbuilding, aerospace wear-resistant parts, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The microscopic morphology of the two-dimensional material Ti3AlC2 before and after etching in the embodiment of the present invention and the comparative example; Figure 2 It is a voltage-current-time curve diagram of the samples in the plasma electrolytic oxidation process of the embodiments of the present invention and the comparative examples; Figure 3 The macroscopic morphology of the three samples, TC6 substrate, TC6-PEO, and PEO-Ti3C2, and the microscopic morphology of the TC6-PEO coating; Figure 4 It is the surface morphology and microscopic morphology of three samples: TC6 matrix, TC6-PEO, and PEO-Ti3C2; Figure 5 It is the Vickers hardness of three samples: TC6 matrix, TC6-PEO, and PEO-Ti3C2; Figure 6 The two-dimensional and three-dimensional profiles and wear information of TC6 matrix, TC6-PEO, PEO-Ti3C2 and steel ball after wear; Figure 7 The friction coefficient and average friction coefficient of three samples, TC6 matrix, TC6-PEO, and PEO-Ti3C2, under 1N-0.2dm / s dry friction conditions; Figure 8 The morphology of the wear tracks and the corresponding wear types of the three samples after friction tests: TC6 matrix, TC6-PEO, and PEO-Ti3C2; Fig. 9 The cross-sectional profiles of TC6-PEO and PEO-Ti3C2 samples before and after wear; Fig.10 It is the three-dimensional profile of the PEO-Ti3C2 sample after wear test at 3N load and 0.15dm / s, 0.20dm / s, 0.25dm / s and 0.3dm / s respectively; Fig.11 The wear track profile curves of PEO-Ti3C2 samples after wear tests at 3N load and 0.15dm / s, 0.20dm / s, 0.25dm / s and 0.3dm / s, respectively; Fig.12 is the average friction coefficient of TC6 matrix, TC6-PEO, and PEO-Ti3C2 samples under loads of 1N, 3N, 5N, and 7N and 0.2dm / s; Fig.13 is the average friction rate of TC6 matrix, TC6-PEO, and PEO-Ti3C2 samples under 1N, 3N, 5N, and 7N loads and 0.2dm / s respectively;

[0037] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0038] Example 1

[0039] The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface comprises the following steps:

[0040] In step 1, the surface of the titanium alloy grinding disc is pretreated, including polishing the surface of the titanium alloy grinding disc with silicon carbide sandpaper and flannel. Specifically, the surface of the titanium alloy grinding disc is first polished with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then polished with 2000 mesh flannel. The sandpaper is silicon carbide sandpaper, so that the surface is free of foreign matter and smooth.

[0041] In the electrolyte prepared in step 2, the concentration of sodium hexametaphosphate is 12 g / L, the concentration of sodium hydroxide is 2.5 / L, the concentration of sodium silicate is 10 / L, the concentration of ammonium metavanadate is 2.5 g / L, and the concentration of potassium fluoride is 0.5 g / L. The stirring speed is 800 r / min and the stirring time is 25 min.

[0042] In step 3, plasma electrolytic oxidation is carried out in constant current control mode, the positive current and negative current are set to 1.3 A and 0.2 A respectively, the pulse frequency is set to 400 Hz, the positive and negative duty cycles are both 12%, and the reaction time is set to 13 min to obtain a grinding disc with a PEO coating on the surface.

[0043] In step 4, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

[0044] Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface;

[0045] Example 2

[0046] The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface comprises the following steps:

[0047] In step 1, the surface of the titanium alloy grinding disc is pretreated, including polishing the surface of the titanium alloy grinding disc with silicon carbide sandpaper and flannel. Specifically, the surface of the titanium alloy grinding disc is first polished with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then polished with 2000 mesh flannel. The sandpaper is silicon carbide sandpaper, so that the surface is free of foreign matter and smooth.

[0048] In the electrolyte prepared in step 2, the concentration of sodium hexametaphosphate is 14 g / L, the concentration of sodium hydroxide is 3.0 g / L, the concentration of sodium silicate is 12 g / L, the concentration of ammonium metavanadate is 3.0 g / L, and the concentration of potassium fluoride is 0.8 g / L. The stirring speed is 900 r / min and the stirring time is 26 min.

[0049] In step 3, plasma electrolytic oxidation is carried out in a constant current control mode, the positive current and negative current are set to 1.5 A and 0.3 A respectively, the pulse frequency is set to 500 Hz, the positive and negative duty cycles are both 18%, and the reaction time is set to 15 min to obtain a grinding disc with a PEO coating on the surface.

[0050] In step 4, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

[0051] Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface;

[0052] Example 3

[0053] The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface comprises the following steps:

[0054] In step 1, the surface of the titanium alloy grinding disc is pretreated, including polishing the surface of the titanium alloy grinding disc with silicon carbide sandpaper and flannel. Specifically, the surface of the titanium alloy grinding disc is first polished with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then polished with 2000 mesh flannel. The sandpaper is silicon carbide sandpaper, so that the surface is free of foreign matter and smooth.

[0055] In the electrolyte prepared in step 2, the concentration of sodium hexametaphosphate is 16 g / L, the concentration of sodium hydroxide is 3.0 g / L, the concentration of sodium silicate is 13 g / L, the concentration of ammonium metavanadate is 3.5 g / L, and the concentration of potassium fluoride is 0.9 g / L. The stirring speed is 1000 r / min and the stirring time is 27 min.

[0056] In step 3, plasma electrolytic oxidation is carried out in a constant current control mode, the positive current and negative current are set to 1.6 A and 0.4 A respectively, the pulse frequency is set to 550 Hz, the positive and negative duty cycles are both 20%, and the reaction time is set to 14 min to obtain a grinding disc with a PEO coating on the surface.

[0057] In step 4, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

[0058] Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface.

[0059] Example 4

[0060] The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface comprises the following steps:

[0061] In step 1, the surface of the titanium alloy grinding disc is pretreated, including polishing the surface of the titanium alloy grinding disc with silicon carbide sandpaper and flannel. Specifically, the surface of the titanium alloy grinding disc is first polished with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then polished with 2000 mesh flannel. The sandpaper is silicon carbide sandpaper, so that the surface is free of foreign matter and smooth.

[0062] In the electrolyte prepared in step 2, the concentration of sodium hexametaphosphate is 15 g / L, the concentration of sodium hydroxide is 3.5 g / L, the concentration of sodium silicate is 15 g / L, the concentration of ammonium metavanadate is 4.5 g / L, and the concentration of potassium fluoride is 1.0 g / L. The stirring speed is 1100 r / min and the stirring time is 28 min.

[0063] In step 3, a constant current control mode is used for plasma electrolytic oxidation, the positive current and the negative current are set to 1.6 A and 0.4 A respectively, the pulse frequency is set to 600 Hz, the positive and negative duty cycles are both 22%, and the reaction time is set to 15 min.

[0064] In step 4, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

[0065] Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface.

[0066] The surface morphology of Ti3C2 samples prepared by etching-ultrasonic cleaning-purification in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 was observed, and their organizational structures were shown in Table 1. Figure 1 As can be seen from these figures, the nanoparticles obtained by etching, ultrasonic cleaning and final purification in Comparative Examples 1, 2, 3 and 4 all have typical layered accordion structures.

[0067] The voltage-current-time parameters of the samples prepared before and after plasma electrolytic oxidation in Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 were recorded and processed. Figure 2 ,from Figure 2 It can be seen that in the constant current mode, the plasma electrolytic oxidation arc-violent discharge process is very stable;

[0068] The surface morphology, micromorphology and Vickers hardness of Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 after plasma electrolytic oxidation and deposition were tested. Figure 3 , 4 As shown in Figure 5, the plasma electrolytic oxidation coating is dense and uniform, with a typical microporous structure. Compared with the substrate, the friction coefficient is increased, but it can provide an ideal storage space for nano-lubricating particles, and the hardness is doubled. After depositing Ti3C2 nanoparticles, the morphology of the sample is flatter, but the surface hardness is reduced.

[0069] The wear of the TC6 titanium alloy grinding disc substrate, as well as the samples and steel balls prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 under different loads was measured. The measurement results are shown in Figure 6 and Figure 7From the two figures, it can be seen that the wear of the TC6 alloy substrate is quite serious. The three-dimensional profile shows that there are obvious pear grooves on the surface and the volume loss of the steel ball is about 7.8×10 -4 mm 3 As the number of cycles increases, the average friction coefficient of the TC6 titanium alloy grinding disc substrate increases slightly at first, then the fluctuation decreases and finally stabilizes (0.4). The wear condition of the TC6-PEO sample is greatly improved under 1N-0.2dm / s. A large amount of wear debris accumulates on the surface of the steel ball. Although the friction coefficient increases, the wear volume is reduced to 1.6×10 -4 mm 3 , The wear mode at this time is mainly abrasive wear. The friction coefficient of the PEO-Ti3C2 sample has dropped to the same level as the substrate (0.4), but the overall trend is a fluctuating increase. The friction coefficient of the TC6-PEO sample has dropped by 45.5%. This is because as the number of friction cycles increases, the lubricating film on the surface is constantly decomposed and reorganized, and the glaze layer on the scratches is constantly compacted and filled with wear debris, resulting in fluctuations in the friction coefficient. However, at this time, the wear rate of both the steel ball and the sample surface has dropped significantly, especially the contact surface contour structure of the steel ball is complete.

[0070] Figure 8 The cross-sectional profiles of the three samples after wear are shown. Figure 8 It can be seen that the surface of the TC6 titanium alloy grinding wheel substrate is severely worn, with adhesive wear and plowing wear being the most serious. This is the result of repeated rolling of the wear debris produced by wear under the action of grinding force. The TC6-PEO sample coating exhibits good wear resistance when subjected to load. Stratification and abrasive accumulation on the edge occur on the surface due to abrasive wear. The friction coefficient is large, but the wear resistance is always better than that of the substrate. The PEO-Ti3C2 sample coating exhibits excellent wear resistance throughout the wear cycle. After lateral comparison, it is found that only a discontinuous glaze layer produced by abrasive wear and sliding wear appears on the surface of Example 1, indicating that the friction-reducing and lubricating interface structure customized on the titanium alloy surface using the method of the present invention has good tribological properties.

[0071] Fig. 9 The cross-sectional profiles of TC6-PEO and PEO-Ti3C2 samples before and after wear are shown. There is a clear boundary between the collective and the PEO coating, and obvious stratification occurs. At the same time, the structure remains stable after wear, except that a composite interface rich in Ti3C2 nanoparticles and TiO2 appears on the surface with a thickness of about 13.80 microns.

[0072] Fig.10 and Fig.11The wear track contour curves and three-dimensional wear profile morphologies of the PEO-Ti3C2 sample under 3N load and different rates are shown respectively. Macroscopically, a lubricating layer appeared on the scratches of the sample at different rates. Combined with the contour track curve, it can be found that abrasive accumulation appeared on the edge of the track, which indicates that the low shear force Ti3C2 nanoparticles play an obvious role in reducing friction and lubrication. The main wear modes of the samples under the four conditions are sliding wear and abrasive wear.

[0073] The wear conditions of three samples, TC6, TC6-PEO and PEO-Ti3C2, were tested at 0.2dm / s and under different load conditions. Through cross-comparison, the TC6 alloy grinding wheel substrate was severely worn in the range of 1N-7N. Both the steel ball and the sample surface experienced great wear, but the friction coefficient first increased and then decreased and stabilized at around 0.39. The wear rate of the TC6-PEO sample increased with the increase of load. Due to the change in wear mode, the friction coefficient maintained a downward trend in the range of 1N-7N, and the wear rate was an order of magnitude lower than the average of the substrate. The PEO-Ti3C2 sample always maintains a low friction coefficient (0.4) under variable load conditions. At the same time, the cross-comparison of the substrate and the PEO sample wear rate is significantly reduced. At 1N, the wear rate is about 16 times lower than that of the base. In other words, the tribological performance of the bone-skin interface structure customized on the titanium alloy surface by plasma electrolytic oxidation and two-dimensional Ti3C2 nanoparticles is excellent. The variable speed and variable load experiments verify the reliability of the structure. Macroscopic tests and onlooker characterizations confirm the synergistic effect of Ti3C2 skin and hard PEO coating in the friction reduction and lubrication effect. From a technical point of view, the surface characteristics and tribological properties of the sample coatings prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 are excellent. This simple and economical surface strengthening technology can promote the wider application of titanium alloys as structural materials, and achieve extremely low wear rates and excellent structural stability in dry friction and wear. This has a far-reaching impact on the field of contact tribology. In addition, future advances can also customize the design of the friction interface according to specific application scenarios and requirements. In other words, the in-situ synthesis of high-stability ceramic coatings solves the long-term limitation of poor wear resistance of alloy substrates in the process of technology promotion. This stable anti-friction lubrication interface structure has the effect of anti-wear and anti-friction lubrication. In the long run, as the high-end manufacturing industry continues to increase its requirements for durability, the interface structure of the synergistic effect of two-dimensional material nano-coating and PEO technology provides a promising way to improve the friction performance of titanium alloys and reduce energy consumption. This has important research significance and economic value.

Claims

1. A method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface, characterized in that: The following steps are involved: Step 1, pre-treating the surface of the titanium alloy grinding disc; Step 2, sodium silicate, sodium hexametaphosphate, sodium bicarbonate, ammonium metavanadate and potassium fluoride are placed in water and stirred until all dissolved to obtain an electrolyte; Step 3, placing the TC6 grinding disc obtained in step 1 in the electrolyte obtained in step 2, and performing plasma electrolytic oxidation in a constant current control mode to obtain a grinding disc with a PEO coating on the surface; Step 4, etching Ti3AlC2 in hydrofluoric acid, then repeatedly washing with plasma water, dispersing the purified Ti3C2 nanoparticles in a propanol solution, and preparing a dispersion after ultrasonic dispersion; Step 5, coating the Ti3C2 nanoparticles prepared in step 4 onto a horizontally placed titanium alloy grinding disc to obtain a titanium alloy grinding disc PEO-Ti3C2 having a Ti3C2 coating and a PEO coating on the surface.

2. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: In the step 1, the surface of the titanium alloy grinding disc is pretreated, including grinding the surface of the titanium alloy grinding disc with sandpaper and flannel to make the surface free of foreign matter and smooth.

3. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: The step 1 specifically includes first grinding the surface of the titanium alloy grinding disc with 600 mesh, 800 mesh, and 1000 mesh sandpaper in sequence, and then grinding the surface of the titanium alloy grinding disc with 2000 mesh flannel cloth, wherein the sandpaper is silicon carbide sandpaper to make the surface free of foreign matter and smooth.

4. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: The sandpaper is silicon carbide sandpaper.

5. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: The concentration of sodium hexametaphosphate in the electrolyte I is 12-18 g / L, the concentration of sodium hydroxide is 2.5-3.5 g / L, the concentration of sodium silicate is 10-15 g / L, the concentration of ammonium metavanadate is 2.5-4.5 g / L, and the concentration of potassium fluoride is 0.5-1.0 g / L.

6. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: The stirring speed is 800-1100 r / min, and the stirring time is 25-30 min.

7. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: In step 4, the plasma electrolytic oxidation is carried out in a constant current control mode, and the positive current and the negative current are set to 1.3-1.7A and 0.1-0.5A / dm respectively. 2 The pulse frequency is set to 400Hz~600Hz, the positive and negative duty cycles are both 12%~22%, and the response time is set to 13min~16min.

8. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: In step 5, 6 g of Ti3AlC2 powder (particle size - 40 nm) was added to 55-65 ml of 40% pure hydrofluoric acid, reacted for 3-5 hours, and then washed with deionized water until the pH was close to 6.0-7.

5. Then, the suspension was centrifuged at 2500 rpm for 30 minutes, and the washing and centrifugation process was repeated three times to separate and purify the powder.

9. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: In the step 5, the prepared 1 mg / ml dispersion solution is evenly coated on the surface of the horizontally placed TC6-PEO sample by drop casting.

10. The method for constructing a friction-reducing and lubricating interface structure on a titanium alloy surface according to claim 1, characterized in that: The titanium alloy grinding disc is made of TC6 alloy.