Multifunctional intelligent protection and danger sensing nanofiber fabric, preparation method thereof and wireless sensing transmission system

By using composite triboelectric nano yarns and nanosilver modified nano-aramid film barrier layers in nanofiber fabrics, the high temperature resistance, corrosion resistance and self-drive problems of nanofiber fabrics are solved, and high chemical stability and protection functions are achieved , and combine it with wireless sensing system to realize remote information monitoring.

CN119041074APending Publication Date: 2024-11-29JIANGSU TANGWEAR IND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310612846.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing nanofiber fabrics cannot withstand high temperature and corrosion resistance, and are difficult to meet the needs of flexibility, lightness, washing, wear resistance and self-drive functions, and there are problems of waste of resources and environmental pollution.

Method used

Using composite triboelectric nano yarns and nanosilver modified nano-aramid film barrier layers, multifunctional intelligent protection and hazard sensing nanofiber fabrics are prepared through electrospinning process, including carbon nanofiber cores and Ag0@Mxene doped SiO2 nanometers The fibers, combined with the silver ion-modified nano-aramid film barrier layer, form conductive paths and barrier layers, and realize self-driven sensing function.

Benefits of technology

It realizes the high chemical stability, flame retardant properties, antibacterial and anti-viral functions of nanofiber fabrics, can withstand high temperature fire fields and strong acid and alkali environments, has good triboelectric properties and durability, and is also connected to wireless sensing systems. Combined, remote information monitoring is realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041074A_ABST
    Figure CN119041074A_ABST
Patent Text Reader

Abstract

The invention relates to a multifunctional intelligent protection and danger sensing nanofiber fabric, a preparation method thereof and a wireless sensing transmission system comprising the multifunctional intelligent protection and danger sensing nanofiber fabric. The nano-fiber fabric comprises a plain bearing layer and a nano-silver-modified nano aramid film barrier layer covering the surface of the plain bearing layer, wherein the surface of the plain bearing layer is coated with the nano-silver-modified nano aramid film barrier layer; wherein the plain bearing layer is formed by weaving composite triboelectric nano-yarns, and the composite triboelectric nano-yarns comprise carbon nano-fiber core yarns and SiO2 nano-fibers doped with Ag0 and Mxene, and the outer layers of the carbon nano-fiber core yarns are wrapped with the SiO2 nano-fibers. The nanofiber fabric not only has good flexibility and wearing comfort, but also has antibacterial, antiviral, good flame retardant and acid and alkali resistant functions, the flame retardant property of the nanofiber fabric reaches the V0 level through a vertical combustion method, the nanofiber fabric can tolerate a sodium hydroxide solution with the concentration being 30% and a sulfuric acid solution with the concentration being 80%, meanwhile, the nanofiber fabric can sense high temperature and strong acid and alkali solutions, and the nanofiber fabric has the advantages of being good in flame retardant property and good in acid and alkali resistance. And the method is suitable for high-risk environment individual protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of intelligent sensing textile fabrics, and in particular relates to a multifunctional intelligent protection and danger perception nanofiber fabric, a preparation method thereof, and a wireless sensing transmission system comprising the same. Background Art

[0002] Thanks to the advancement and widespread application of artificial intelligence and Internet of Things technologies, the rise of 5G communication technology, and the miniaturization of electronic components, the smart textile market has developed rapidly. According to the latest report from market research company Marketsand Markets, the global smart textile market size is about US$2.3 billion in 2021 and will reach US$6.6 billion in 2026, with an average annual compound growth rate of 23.2%. In recent years, with the rapid development of modern industries, safety accidents such as fires and leakage of high-risk chemicals have occurred frequently, and there is an urgent need to develop smart sensing textiles with both individual protection functions (such as flame retardant, acid and alkali resistance, etc.) and hazard warning functions. However, existing traditional smart sensing textiles usually integrate electronic components into the surface of the fabric, have poor high temperature resistance and corrosion resistance, and are difficult to meet the requirements of flexibility, lightness, and washability. In addition, the integrated electronic components often contain heavy metals such as mercury and lead, and often require additional external power supply devices such as batteries and supercapacitors, resulting in problems such as frequent charging and safety. Therefore, there is an urgent need to develop flexible sensing textiles that are safe and reliable, flexible and thin, washable and wear-resistant, and have both self-driving and personal protection functions. This is also the future development direction of flexible wearable smart devices.

[0003] In recent years, researchers have developed flexible fiber sensors, yarn-bound sensors, and flexible textiles to address the issues of flexibility and thinness. For example, Qiang Gao's team at Fudan University used dry spinning to make biopolymer P 3 HB 4HB and conductive antimony-containing tin oxide wrapped titanium dioxide nanoparticles prepared fibers that can be stretched more than 700%, and the fibers showed good mechanical and electrical reversible properties within a strain range of 420%. Kun Qi et al. used electrospinning technology to wrap nanotube (CNT)-doped PU nanofibers on nickel-plated conductive cotton yarn to obtain a skin-core structure composite yarn, and prepared a network structure pressure sensor through a weaving process, with a high sensitivity of 16.52N-1, a sensing range of 0.003–5N, and a response time of about 0.03s, which can be used for human motion monitoring. However, the above materials are not resistant to high temperatures and corrosion, and have not yet gotten rid of external power supply devices, and there are problems with wear resistance, washability and safety. In response to the waste of resources and environmental pollution caused by frequent battery replacement, domestic and foreign research institutions have successively carried out research on self-driven intelligent sensing textiles. At present, the main research directions of self-driven intelligent sensing textiles are divided into three categories: intelligent piezoelectric textiles, intelligent triboelectric textiles, and intelligent pyroelectric textiles. Among them, piezoelectric and friction applications are the most widely studied. The materials used are mostly II-VI, III-V group nano semiconductors, perovskites, ceramics, etc. such as CdS, GaAs, GaSb, BaTiO3, PZT, etc. The above nano materials are mainly loaded on the fabric by blending, skin-core spinning or coating, but the problems of high temperature resistance and corrosion resistance have not been solved.

[0004] Therefore, there is an urgent need to develop intrinsic piezoelectric / triboelectric fiber textiles with high chemical stability and flame retardant properties. Summary of the invention

[0005] The technical problem to be solved by the present application is that the existing nanofiber fabrics are not resistant to high temperatures and corrosion. To this end, the present invention provides a multifunctional intelligent protection and danger perception nanofiber fabric, and further provides a preparation method thereof and a wireless sensing transmission system including the same.

[0006] The present invention is achieved through the following technical solutions:

[0007] In the first aspect, the present invention provides a multifunctional intelligent protection and danger perception nanofiber fabric, which comprises: a plain weave bearing layer and a nano-aramid film barrier layer coated on the surface of the plain weave bearing layer; wherein the plain weave bearing layer is woven from a composite triboelectric nano yarn, and the composite triboelectric nano yarn comprises a carbon nanofiber core yarn and Ag wrapped around the outer layer of the carbon nanofiber core yarn. 0 @Mxene-doped SiO 2 Nanofibers.

[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned multifunctional intelligent protection and danger perception nanofiber fabric, comprising the following steps:

[0009] Preparing an alkyl silicate (e.g., tetraethyl orthosilicate) / polyacrylonitrile (PAN) composite spinning solution;

[0010] Spinning the alkyl silicate (e.g., tetraethyl orthosilicate) / polyacrylonitrile (PAN) composite spinning solution into yarn to prepare polyacrylonitrile (PAN) composite yarn;

[0011] Preparation of Ag + @MXene doped PAN / alkyl silicate (such as tetraethyl orthosilicate) precursor spinning solution, using the PAN / alkyl silicate (such as tetraethyl orthosilicate) precursor spinning solution to spray the Ag on the surface of the polyacrylonitrile PAN composite yarn + @MXene-doped polyacrylonitrile PAN / alkyl silicate (e.g., tetraethyl orthosilicate) precursor nanofibers to prepare polyacrylonitrile PAN composite core-spun yarn;

[0012] The polyacrylonitrile (PAN) composite core-spun yarn is immersed in a forming agent solution, and then subjected to radiation cross-linking treatment;

[0013] High temperature carbonization to prepare composite triboelectric nano yarns;

[0014] Weaving the composite triboelectric nano yarn into a plain weave load-bearing layer;

[0015] preparing a PMIA spinning solution, and then weaving the PMIA spinning solution into a silver ion-modified nano-aramid film barrier layer;

[0016] The silver ion modified nano-aramid film barrier layer is subjected to a reduction reaction to obtain a nano-silver modified nano-aramid film barrier layer;

[0017] The nano-silver modified nano-aramid film barrier layer is coated on the surface of the plain weave bearing layer to obtain the barrier layer.

[0018] Furthermore, the method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric comprises the following steps:

[0019] S1, adding ultra-high molecular weight polyacrylonitrile PAN (weight average molecular weight of 300000-700000, preferably 400000-500000) into a polar aprotic solvent (for example, a mixed solvent of DMF and DMSO, the mass ratio of dimethylformamide DMF and dimethyl sulfoxide DMSO is 15:1-8:1, preferably 12-8:1, more preferably 10-9:1), stirring until completely dissolved, to prepare a spinning solution of polyacrylonitrile PAN;

[0020] S2, adding alkyl silicate (such as tetraethyl orthosilicate) to the spinning solution of polyacrylonitrile PAN, stirring (preferably high-speed stirring, high-speed stirring refers to stirring at 80-120 r / min), to prepare alkyl silicate (such as tetraethyl orthosilicate) / polyacrylonitrile PAN composite spinning solution;

[0021] S3, spinning the alkyl silicate (such as tetraethyl orthosilicate) / polyacrylonitrile (PAN) composite spinning solution into yarn using an electrostatic spinning process to prepare polyacrylonitrile (PAN) composite yarn;

[0022] S4, adding a soluble silver salt to the alcohol solution of the titanium carbide multilayer nanosheets, (for example, heating, preferably refluxing) to adsorb the silver ions on the surface and between the layers of the titanium carbide, dialyzing and drying, to prepare the titanium carbide multilayer nanosheets Ag adsorbed with silver ions. + @MXene; Ultra-high molecular weight polyacrylonitrile PAN and alkyl silicate (such as tetraethyl orthosilicate) are dissolved in polar aprotic solvent DMF, and then silver ion-adsorbed titanium carbide multilayer nanosheets Ag are added + @MXene, stirring (preferably high-speed stirring, high-speed stirring refers to stirring at 80 to 120 r / min), mixing evenly, and preparing Ag + @MXene-doped PAN / alkyl silicate (e.g., tetraethyl orthosilicate) precursor spinning solution; using the PAN / tetraethyl orthosilicate precursor spinning solution to spray the Ag on the surface of the polyacrylonitrile PAN composite yarn through an electrospinning process + @MXene-doped polyacrylonitrile PAN / alkyl silicate (e.g., tetraethyl orthosilicate) precursor nanofibers (PAN composite yarn with sprayed Ag + @MXene-doped PAN / TES mass ratio 1:0.1~1:0.8, Ag + @The mass of MXene-doped PAN / ethyl orthosilicate is 10% to 80% relative to the PAN composite yarn) to prepare polyacrylonitrile PAN composite core-spun yarn;

[0023] S5, after being drawn step by step, the polyacrylonitrile PAN composite core-spun yarn is immersed in a forming agent solution (3wt% to 25wt%, further 10 to 20wt%; the solvent for dissolving the forming agent can be water, and the forming agent can be selected from one or more of butene acid, maleic acid, methyl fumaric acid, etc.) (for example, an ethanol solution of maleic acid with a mass fraction of 20% or an ethanol solution of methyl fumaric acid with a mass fraction of 18%), rolled dry, dried, and finally baked (for example, rolled dry (liquid rolling rate 30-80%, preferably 60%), then dried at 60-100°C, preferably 80°C, for 10-60min, preferably 30min, and finally baked at 100-130°C, preferably 110-120°C, for 5-30min, preferably 10min), and then subjected to gamma ray (must be gamma ray with sufficiently high energy) radiation cross-linking treatment; step-by-step drawing and oriented crystallization can improve mechanical properties;

[0024] S6, the polyacrylonitrile PAN composite core-spun yarn after radiation cross-linking treatment (for example, under nitrogen atmosphere and tension, the specific method of applying tension is as follows: the polyacrylonitrile PAN composite core-spun yarn is wound on an elastic bracket, and the tension can be adjusted by adjusting the length of the bracket) is subjected to high-temperature carbonization, and the polyacrylonitrile PAN composite core-spun yarn is transformed into a carbon nanofiber core yarn after high-temperature carbonization, Ag + @MXene-doped polyacrylonitrile PAN / alkyl silicate (e.g., tetraethyl orthosilicate) precursor nanofibers converted to Ag 0 @Mxene-doped SiO 2 The nanofibers are wrapped in the outer layer of the carbon nano core yarn, and the polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofibers to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn; the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a composite triboelectric nano yarn;

[0025] S7, weaving the composite triboelectric nano yarn into a plain weave load-bearing layer;

[0026] S8, preparing a PMIA spinning solution, and then using the PMIA spinning solution to prepare a silver ion-modified nano-aramid film barrier layer by an electrospinning process;

[0027] S9, the silver ion modified nano-aramid film barrier layer is subjected to a reduction reaction to obtain a nano-silver modified nano-aramid film barrier layer;

[0028] S10. The nano-aramid film barrier layer modified with nano-silver is coated on the surface of the plain weave bearing layer by electrostatic spraying (the spraying voltage is 11KV and the spraying distance is 15cm) to obtain a multifunctional intelligent protection and danger-sensing nanofiber fabric.

[0029] Furthermore, in the method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric, in step S1, the weight average molecular weight of the ultra-high molecular weight polyacrylonitrile is 300,000-700,000, preferably 400,000-500,000, and is preferably prepared by gamma ray in-situ irradiation polymerization; and / or,

[0030] In step S1, the polar aprotic solvent is selected from at least one of dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and sulfolane, preferably a mixed solution of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), preferably, the mass ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is 15:1 to 8:1, preferably 12 to 8:1, more preferably 10 to 9:1; and / or,

[0031] In step S1, the mass concentration of ultra-high molecular weight polyacrylonitrile in the spinning solution of polyacrylonitrile PAN is 5-18%, preferably 7-15%, and more preferably 8-12%.

[0032] Furthermore, in the method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric, in step S2, the alkyl silicate is selected from at least one of tetraethyl orthosilicate, methyl orthosilicate, and butyl orthosilicate, preferably tetraethyl orthosilicate; and / or,

[0033] In step S2, the amount of alkyl silicate added is 0.2-5% of the mass of ultra-high molecular weight polyacrylonitrile, preferably 1-3%, more preferably 1.5-2%; and / or,

[0034] In step S3, in the electrospinning process, the double-nozzle electrospinning voltage is 5-20 kV, preferably 8-15 kV; the spinning speed is 0.01-0.5 ml / h, preferably 0.08-0.22 ml / h; the distance between the spinning needle and the bell mouth is 5-20 cm, preferably 10-15 cm, and more preferably 12 cm; the bell mouth speed is 50-150 r / min, preferably 80-130 r / min, and more preferably 85-125 r / min; the receiving shaft speed is 0.01-5 r / min, preferably 0.1-3 r / min, and more preferably 0.2-3 r / min.

[0035] Furthermore, in the method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric, in step S4, the soluble silver salt is selected from at least one of silver acetate and silver tartrate, preferably silver acetate; silver acetate and silver tartrate are soluble in organic solvents and are compatible with tetraethyl orthosilicate and the like; and / or,

[0036] In step S4, the mass ratio of the soluble silver salt to the titanium carbide multilayer nanosheets is 0.1:10 to 3:10, preferably 0.5:10 to 2:10, and more preferably 1:10, calculated as silver ions; and / or

[0037] In step S4, the alkyl silicate is selected from at least one of ethyl orthosilicate, methyl orthosilicate and butyl orthosilicate, preferably ethyl orthosilicate; and / or,

[0038] In step S4, the mass ratio of ultra-high molecular weight polyacrylonitrile PAN to alkyl silicate is 1:5 to 1:30, preferably 1:10 to 1:20, more preferably 1:15; and / or,

[0039] In step S4, the polar aprotic solvent is selected from at least one of dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and sulfolane, preferably dimethylformamide (DMF); and / or,

[0040] In step S4, the mass ratio of PAN / alkyl silicate to the polar aprotic solvent is 10-25%:1, preferably 15-20%:1; and / or,

[0041] In step S4, the silver ion adsorbed titanium carbide multilayer nanosheet Ag + The mass ratio of @MXene to PAN / alkyl silicate is 1-30%:1, preferably 4-25%:1, preferably 5-20%:1, preferably 8-15%:1; and / or,

[0042] In step S4, in the electrospinning process, the receiving voltage is 10-50 kV, preferably 15-35 kV, the distance between the needle and the bell mouth is 10-25 cm, preferably 16-22 cm, the spinning speed is 0.05 ml / min-0.3 ml / min, preferably 0.10 ml / min-0.20 ml / min; the bell mouth speed is 70 r / min-150 r / min, preferably 90-130 r / min; the winding roller speed is 0.1 r / min-5 r / min, preferably 0.15-2.6 r / min.

[0043] Furthermore, in the method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric, in step S5, the polyacrylonitrile PAN composite core-spun yarn is subjected to three-stage drafting, the first-stage drafting multiple is 1.5-1.8, the second-stage drafting multiple is 0.5-1.2, and the third-stage drafting multiple is 0.3-0.5; and / or,

[0044] In step S5, the molding agent is selected from at least one of crotonic acid, maleic acid, and methyl fumaric acid, preferably maleic acid or methyl fumaric acid, and more preferably an ethanol solution of maleic acid with a mass fraction of 20%; and / or,

[0045] In step S5, the radiation source of the gamma ray radiation cross-linking treatment is 60 Co, radiation dose is 5~13×10 - 5 rad / s; and / or,

[0046] In step S6, high temperature carbonization is performed in a nitrogen atmosphere under tension, wherein the carbonization temperature of the high temperature carbonization is 600-1500° C., preferably 600-1000° C., more preferably 800° C.; the tension is 0.1-30N, preferably 0.8-2.6N; and / or,

[0047] In step S7, the composite triboelectric nano yarn is warp yarn and weft yarn, the weave structure is 1 / 1 plain weave, the warp density of the fabric is 20 to 150 strands / inch, preferably 30 to 78 strands / inch; the weft density is 10 to 70 strands / inch, preferably 20 to 68 strands / inch.

[0048] Furthermore, in the preparation method of the multifunctional intelligent protection and danger perception nanofiber fabric, in step S8, the PMIA spinning solution is prepared according to the following method: PMIA short fibers (length 35 mm-50 mm, diameter 5-30 microns) are cut into pieces (diameter less than 0.1 mm), ultrasonically treated in ethanol (e.g., ultrasonically treated for 10 to 60 minutes, preferably 20 to 40 minutes), and then ultrasonically treated in deionized water (e.g., ultrasonically treated for 10 to 60 minutes, preferably 20 to 40 minutes), and dried to obtain treated PMIA short fibers; the treated PMIA short fibers are immersed in a silver ion / DMAC solution (silver ion / DMA after immersion). C solution, the mass concentration of the treated PMIA staple fibers is 6% to 15%), the mass ratio of silver ions to the treated PMIA staple fibers is 2:1000 to 10:1000, preferably 4:1000 to 8:1000), and expanded at 30-80°C, preferably 60°C, for 0.5-5 hours, preferably 2 hours, and then LiCl is added to the silver ion / DMAC solution (the mass ratio of PMIA to LiCl is (5-15): (1-10), preferably 9:6), stirred at 30-80°C, preferably 60°C, and finally ultrasonically treated (for example, ultrasonically treated for 0.5 to 2 hours, preferably 1 hour) to obtain a PMIA spinning solution; and / or,

[0049] In step S8, in the electrospinning process, the spinning voltage is 5 to 50 kV, preferably 12 to 20 kV; the spinning speed is 0.01 to 0.3 ml / h, preferably 0.05 to 0.2 ml / h; the distance between the spinning needle and the receiving roller is 10 to 30 cm, preferably 15 to 25 cm; the roller speed is 10 to 150 r / min, preferably 30 to 90 r / min; and / or,

[0050] In step S9, the silver ion modified nano-aramid film barrier layer is immersed in an aqueous solution of sodium borohydride with a mass concentration of 0.01% to 1% for 10 to 150 minutes, preferably 30 to 120 minutes, to reduce the silver ions to nano-silver, to prepare a nano-aramid film barrier layer modified with nano-silver, and then immersed in an ethanol solution for 20 to 80 minutes, preferably 40 to 60 minutes. The concentration of the sodium borohydride solution should be low, otherwise the reaction will be too fast.

[0051] Furthermore, in the preparation method of the multifunctional intelligent protection and danger perception nanofiber fabric, after step S10, the following step of performing surface hydrophobic treatment on the multifunctional intelligent protection and danger perception nanofiber fabric is further included: S11, impregnating the multifunctional intelligent protection and danger perception nanofiber fabric in a fluorine-containing finishing agent (preferably a C4 fluorine-containing polymer, such as 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 3M three-proof finishing agent PM-3622, PM-3662 / 3660, etc.) in an ethanol solution (for example, the mass concentration of the fluorine-containing finishing agent in the ethanol solution of the fluorine-containing finishing agent is 1-15%, preferably 1-5%, more preferably 1-3%), the bath ratio is 1:30-1:100, preferably 1:50; then take out and roll dry, the rolling rate is 10-90%, preferably 20%-40%; steam fumigation treatment for 10-60min, preferably 30min, then drying at 60-80℃ for 20-50min, and finally baking at 110-140℃ for 10-30min.

[0052] Furthermore, in step S10, the thickness of the nano-aramid film barrier layer modified with nano-silver can be 40-80 microns, preferably 50-70 microns, further 55-65 microns, and more preferably about 60 microns.

[0053] In a third aspect, the present invention provides a multifunctional intelligent protection and danger perception nanofiber fabric prepared by the above preparation method.

[0054] Preferably, the hydrostatic pressure resistance of the multifunctional intelligent protection and danger perception nanofiber fabric is greater than 5000 mmH 2 O, for example, up to 8780mmH 2 O, moisture permeability>8000g / (m 2D), vertical combustion flame retardancy reaches V0 level, and the single finger touch voltage at room temperature can reach up to 30V.

[0055] In a fourth aspect, the present invention provides a wireless sensing transmission system, comprising the above-mentioned multifunctional intelligent protection and danger perception nanofiber fabric or the multifunctional intelligent protection and danger perception nanofiber fabric prepared by the above-mentioned preparation method.

[0056] Preferably, the wireless sensing transmission system comprises the above-mentioned multifunctional intelligent protection and danger perception nanofiber fabric or the multifunctional intelligent protection and danger perception nanofiber fabric prepared by the above-mentioned preparation method and a wireless signal collector.

[0057] The technical solution of the present invention has the following advantages:

[0058] (1) The multifunctional intelligent protection and danger perception nanofiber fabric of the present invention not only has good flexibility and wearing comfort, but also has a hydrostatic pressure resistance greater than 5000 mmH 2 O, moisture permeability>8000g / (m 2 D), and it has antibacterial and antiviral, good flame retardant, acid and alkali resistance functions. Its flame retardant performance reaches V0 level by vertical combustion method, and it can withstand 30% sodium hydroxide solution and 80% or even 98% sulfuric acid solution;

[0059] (2) The multifunctional intelligent protection and danger sensing nanofiber fabric of the present invention is woven into a finished product with an area of ​​0.5cm*0.5cm~1cm*1cm, which is integrated into the elbow or abdomen. When entering a high-temperature fire environment, the elbow bending voltage signal increases by 137%, and the hand-clapping fabric sensing signal increases by more than 9 times. It can sense high-temperature fires and can be used for high-temperature fire energy collection and high-temperature risk detection; it can generate different induced voltage signals when in contact with different acids and alkalis, can sense strong acid and strong alkali solutions, can be used for acid and alkali exposure risk detection, and is suitable for individual protection applications in high-risk environments;

[0060] (3) The multifunctional intelligent protection and danger sensing nanofiber fabric of the present invention has a contact separation friction test, and the test results show that the voltage is 20.8-23V and the current can reach 218-230nA, so the calculated electric power can reach 9.07-10.58mW / m 2 , after 3000 times of touch pressure, the induced voltage increased slightly, and the triboelectric performance had high durability and stability;

[0061] (4) The multifunctional intelligent protection and danger perception nanofiber fabric of the present invention can be combined with a wireless signal collector to form a wireless sensor transmission system, which can realize remote information monitoring. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0063] Figure 1 (a) and (b) are Ag0@Mxene-doped SiO prepared in Example 1. 2 Photographs and SEM images of nanofiber (sheath)-carbon nanofiber (core) nano-core yarn; Figure 1 (c) Utilization for the embodiment Figure 1 (a) The finished product of the multifunctional intelligent protection and danger perception nanofiber fabric prepared by weaving the prepared nano core-spun yarn;

[0064] Figure 2 (a) and (b) are graphs of the friction-induced (a) voltage and (b) current generated by the multifunctional intelligent protection and hazard perception nanofiber fabric and PTFE-coated fabric at a contact frequency of 0.9 Hz in the contact-separation friction experiment;

[0065] Figure 3 (a) is a schematic diagram of a wireless intelligent hazard perception system composed of the prepared intelligent textile (i.e., the multifunctional intelligent protection and hazard perception nanofiber fabric prepared in Example 1) and a wireless data acquisition card (power supply required);

[0066] Figure 3 (b) In order to integrate the corresponding intelligent hazard perception system into the chemical protective clothing, the hands continuously tap the intelligent fabric, and the computer can receive the corresponding signal through wireless WIFI, thereby realizing the perception of the dangerous environment;

[0067] Figure 4 The test results of the antibacterial experiment are as follows: Figure 4 (a) is the Escherichia coli colonies in the plate count culture dish; Figure 4 (b) Staphylococcus aureus in a plate count culture dish. The results show that no bacteria grew on both plates, indicating that it has super antibacterial properties;

[0068] Figure 5 The test results of liquid repellency in the acid and alkali proof experiment show that the liquid repellency of the multifunctional intelligent protection and danger perception nanofiber fabric to water, 30% sodium hydroxide solution, 40% nitric acid solution, and 80% sulfuric acid solution are all over 97%, exceeding the highest level of the national standard;

[0069] Figure 6 This is the test result of the strong acid and strong alkali perception experiment. Figure 6The data is the pulse induced voltage generated by the multifunctional intelligent protection and danger perception nanofiber fabric repeatedly contacting 80% sulfuric acid solution and 30% sodium hydroxide solution at a frequency of about 1.2Hz. The results show that the fabric can generate a peak voltage of nearly 8V when contacting 80% sulfuric acid solution, and a peak voltage of nearly 17V when contacting 30% hydroxide solution. Therefore, the acidity and alkalinity of the solution can be distinguished by the strength of the voltage signal generated by contact with the liquid;

[0070] Figure 7 (a) and Figure 7 (b) are the results of the high-temperature fire scene perception experiment, (a) is the pulse voltage generated by continuously bending the elbow in normal temperature environment and fire environment; (b) is the pulse voltage generated when the hand touches the abdominal fabric in normal temperature environment and fire environment. The results show that when the operator switches from a normal temperature environment to a high temperature environment, the peak voltage increases significantly. The peak voltage generated by bending the elbow increases from about 2V to about 4.7V, and the peak voltage generated by touching the abdominal fabric with the hand increases from about 2V to about 14.3V. The sudden change of this peak voltage can be used for high-temperature fire scene environment perception, and can be used for smart fire scene perception curtains, wall coverings, fire suits, etc. DETAILED DESCRIPTION

[0071] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0072] In the following examples, the electrostatic spinning machine, HZ-SX-01 nano spinning machine, was purchased from Qingdao Nuokang Environmental Protection Technology Co., Ltd., and can also be homemade;

[0073] PMIA refers to aramid, which was purchased from Yantai Taihe New Materials Co., Ltd.;

[0074] Polyacrylonitrile (PAN), customized by China Institute of Radiation Protection (Taiyuan);

[0075] Titanium carbide multilayer nanosheets, CAS number: 12363-89-2, model XFK01-1, purchased from Pioneer Nano;

[0076] Fluoropolymer, Scotchgard PM-3662 / 3660, C4 fluorine series, purchased from 3M Company;

[0077] Ethyl orthosilicate, analytical grade, was purchased from Sinopharm Group;

[0078] PMIA short fibers, 35 mm to 50 mm in length and 5 to 30 μm in diameter, were purchased from Yantai Taihe New Materials Co., Ltd.;

[0079] The wireless signal collector, model VK7015W, was purchased from Shenzhen Weijingyi Electronics Co., Ltd.

[0080] Example 1

[0081] The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric of this embodiment comprises the following steps:

[0082] (1) 9 g of ultra-high molecular weight polyacrylonitrile PAN powder (weight average molecular weight 400,000) was dissolved in 91 g of organic solvent DMF / DMSO solution (DMF / DMSO mass ratio was 9:1), and stirred continuously at room temperature for 24 hours until it was completely dissolved to prepare a spinning solution of polyacrylonitrile PAN;

[0083] (2) adding 0.15 g of tetraethyl orthosilicate to the spinning solution of polyacrylonitrile (PAN), stirring at high speed (100 r / min), to prepare a tetraethyl orthosilicate / PAN composite spinning solution;

[0084] (3) Using an electrospinning machine and an electrospinning process to spin the tetraethyl orthosilicate / PAN composite spinning solution, double nozzle spinning, spinning voltage 15kV; spinning speed 0.2ml / h, the distance between the spinning needle and the bell mouth 12cm; bell mouth speed 100r / min; receiving shaft speed 1.2r / min, to prepare polyacrylonitrile PAN composite yarn;

[0085] (4) Add 0.16 g of silver acetate to 100 ml of 10 mg / ml ethanol solution of titanium carbide multilayer nanosheets (the mass ratio of silver ions to titanium carbide after conversion is 1:10), heat and reflux to adsorb silver ions on the surface and between the layers of titanium carbide, dialyze and dry to prepare silver ion-adsorbed titanium carbide multilayer nanosheets Ag. + @MXene; 2 g of PAN powder and 30 g of tetraethyl orthosilicate were dissolved in 200 g of DMF to obtain a DMF solution of PAN / tetraethyl orthosilicate, and then 1.6 g of Ag was added. + @MXene, high-speed stirring (110r / min stirring), mixing evenly, preparing PAN / ethyl orthosilicate precursor spinning solution; using the PAN / ethyl orthosilicate precursor spinning solution to spray Ag on the surface of the polyacrylonitrile PAN composite yarn through an electrospinning process + @MXene-doped PAN / TES precursor nanofibers (PAN composite yarn with sprayed Ag + @MXene-doped PAN / TES mass ratio 1:0.5, Ag+ @The mass of MXene-doped PAN / ethyl orthosilicate is 50% relative to the PAN composite yarn), the electrospinning process is as follows: receiving voltage 18kV, the distance between the needle and the bell mouth is 18cm, the spinning speed is 0.15ml / min; the bell mouth speed is 110r / min; the winding roller speed is 1.5r / min, and the polyacrylonitrile PAN composite core-spun yarn is prepared;

[0086] (5) The polyacrylonitrile (PAN) composite core-spun yarn was drawn through a first-stage drawing multiple of 1.6 times, a second-stage drawing multiple of 0.6 times, and a third-stage drawing multiple of 0.3 times for step-by-step drawing orientation crystallization to improve the mechanical properties; then, it was immersed in an ethanol solution of maleic acid with a mass fraction of 20%, rolled dry (rolling liquid rate 60%), and then dried at 80°C for 30 minutes, and finally baked at 110°C for 10 minutes; then, a gamma ray radiation source was used as 60 Co was cross-linked by radiation, and the radiation dose was 8×10 -5 rad / s;

[0087] (6) After radiation crosslinking treatment, the polyacrylonitrile PAN composite core-spun yarn was carbonized at high temperature under nitrogen atmosphere and tension. The carbonization temperature was 800℃ and the tension was 2N. After high temperature carbonization, the polyacrylonitrile PAN composite core-spun yarn was transformed into carbon nanofiber core yarn. Ag + @MXene-doped polyacrylonitrile PAN / tetraethyl orthosilicate precursor nanofibers converted to Ag 0 @MXene-doped SiO 2 The nanofibers are wrapped around the outer layer of the carbon nanofiber core yarn. The outer layer of polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofiber to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn; the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a high-strength and high-toughness antibacterial and antiviral composite triboelectric nano yarn (Ag0@MXene-doped SiO 2 Nanofiber (sheath) - carbon nanofiber (core) nano-core yarn);

[0088] (7) Weaving the composite triboelectric nano yarn into a plain bearing layer, using the composite triboelectric nano yarn as the warp and weft, the weave structure adopts a 1 / 1 plain weave, the warp density of the fabric is 70 strands / inch, and the weft density is 60 strands / inch;

[0089] (8) Cut PMIA short fibers (length 35 mm-50 mm, diameter 5-30 μm) into pieces (diameter < 0.1 mm), continuously ultrasonically treat in ethanol for 30 minutes, then continuously ultrasonically treat in deionized water for 30 minutes, and dry to obtain treated PMIA short fibers; immerse the treated PMIA short fibers in a silver ion / DMAC solution (in the silver ion / DMAC solution after immersion, the mass concentration of the treated PMIA short fibers is 10%), the mass ratio between silver ions and the treated PMIA short fibers is 6:1000, and heat at 60 °C for 2 hours. ℃ oven for 2 hours, add LiCl (wherein the mass ratio of PMIA to LiCl is 9:6) to the silver ion / DMAC solution, stir continuously at 60 ℃ to obtain a light yellow solution, and finally ultrasonically treat for 1 hour to prepare a PMIA spinning solution, and then use electrospinning to spin the PMIA spinning solution to prepare a silver ion modified nano-aramid film barrier layer, and spin with 2 needles in a horizontal row. The preparation process is as follows: the multi-nozzle electrospinning voltage is 18 kV, the spinning speed is 0.15 ml / h, the distance between the spinning needle and the receiving roller is 16 cm, and the roller speed is 60 min / r;

[0090] (9) immersing the silver ion-modified nano-aramid film barrier layer in an aqueous solution of sodium borohydride with a mass concentration of 0.05% for 30 minutes to reduce the silver ions to nano-silver, and preparing the nano-aramid film barrier layer modified with nano-silver through a reduction reaction, and then immersing it in an ethanol solution for 60 minutes to fully precipitate Li, Cl and other ions;

[0091] (10) Electrostatic spraying (spraying voltage of 11KV, spraying distance of 15cm) is used to coat the nano-silver modified nano-aramid film barrier layer on the surface of the plain weave bearing layer. The thickness of the nano-aramid film barrier layer is about 60 microns, and a multifunctional intelligent protection and danger perception nanofiber fabric can be obtained;

[0092] (11) The multifunctional intelligent protection and hazard perception nanofiber fabric was immersed in a 3% mass concentration of fluoropolymer ethanol solution with a bath ratio of 1:50; then the fabric was taken out and squeezed to dry with a squeeze rate of 40%, steam fumigated for 30 minutes, dried at 70°C for 30 minutes, and finally baked at 110°C for 10 to 30 minutes.

[0093] The Ag0@Mxene-doped SiO prepared in this example 2 Photographs and SEM images of nanofiber (sheath)-carbon nanofiber (core) nano-core yarns Figure 1 (a) and Figure 1 (b) shows the finished product obtained by weaving. Figure 1 (c) as shown.

[0094] Example 2

[0095] The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric of this embodiment comprises the following steps:

[0096] (1) 8 g of polyacrylonitrile (PAN) powder (weight average molecular weight 500,000) was dissolved in 92 g of organic solvent DMF / DMSO solution (DMF / DMSO mass ratio was 9:1), and stirred continuously at room temperature for 24 hours until it was completely dissolved, thereby preparing a spinning solution of polyacrylonitrile PAN;

[0097] (2) adding 0.16 g of tetraethyl orthosilicate to the spinning solution of polyacrylonitrile (PAN), stirring at high speed (110 r / min), to prepare a tetraethyl orthosilicate / PAN composite spinning solution;

[0098] (3) Using an electrospinning machine and an electrospinning process, the tetraethyl orthosilicate / PAN composite spinning solution was spun, double nozzle spinning, spinning voltage 16kV; spinning speed 0.22ml / h, the distance between the spinning needle and the bell mouth 12cm; bell mouth speed 110r / min; receiving shaft speed 1.4r / min, to prepare polyacrylonitrile PAN composite yarn;

[0099] (4) Add 0.16 g of silver acetate to 100 ml of 10 mg / ml ethanol solution of titanium carbide multilayer nanosheets (the mass ratio of silver ions to titanium carbide after conversion is 1:10), heat and reflux to adsorb silver ions on the surface and between the layers of titanium carbide, dialyze and dry to prepare silver ion-adsorbed titanium carbide multilayer nanosheets Ag. + @MXene; 2 g of PAN powder and 30 g of tetraethyl orthosilicate were dissolved in 200 g of DMF to obtain a DMF solution of PAN / tetraethyl orthosilicate, and then 1.6 g of Ag was added. + @MXene, high-speed stirring (120r / min stirring), mixed evenly, and Ag was prepared + @MXene-doped PAN / ethyl orthosilicate precursor spinning solution; using the PAN / ethyl orthosilicate precursor spinning solution to spray Ag on the surface of the polyacrylonitrile PAN composite yarn through an electrospinning process + @MXene PAN / tetraethyl orthosilicate precursor nanofibers (PAN composite yarn with sprayed Ag + @MXene-doped PAN / TES mass ratio 1:0.2, Ag +@The mass of MXene-doped PAN / ethyl orthosilicate is 20% relative to the PAN composite yarn), and the electrospinning process is as follows: receiving voltage 18kV, the distance between the needle and the bell mouth is 18cm, the spinning speed is 0.15ml / min; the bell mouth speed is 110r / min; the winding roller speed is 1.5r / min, and finally the polyacrylonitrile PAN composite core-spun yarn is prepared;

[0100] (5) The polyacrylonitrile (PAN) composite core-spun yarn was drawn through a first-stage drawing multiple of 1.6 times, a second-stage drawing multiple of 0.6 times, and a third-stage drawing multiple of 0.3 times for step-by-step drawing orientation crystallization to improve the mechanical properties; then, it was immersed in an ethanol solution of maleic acid with a mass fraction of 20%, rolled dry (rolling liquid rate 60%), and then dried at 80°C for 30 minutes, and finally baked at 110°C for 10 minutes; then, a gamma ray radiation source was used as 60 Co was cross-linked by radiation, and the radiation dose was 5×10 -5 rad / s;

[0101] (6) After radiation crosslinking treatment, the polyacrylonitrile PAN composite core-spun yarn was carbonized at high temperature under nitrogen atmosphere and tension. The carbonization temperature was 800℃ and the tension was 2N. After high temperature carbonization, the polyacrylonitrile PAN composite core-spun yarn was transformed into carbon nanofiber core yarn. Ag + @MXene-doped PAN / TES precursor nanofibers converted to Ag 0 @MXene-doped SiO 2 The nanofibers are wrapped around the outer layer of the carbon nanofiber core yarn. The outer layer of polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofiber to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn; the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a composite triboelectric nano yarn;

[0102] (7) Weaving the composite triboelectric nano yarn into a plain bearing layer, using the composite triboelectric nano yarn as the warp and weft, the weave structure adopts 1 / 1 plain weave, the warp density of the fabric is 70 strands / inch, and the weft density is 60 strands / inch;

[0103] (8) Cut PMIA short fibers (length 35 mm-50 mm, diameter 5-30 μm) into pieces (diameter < 0.1 mm), continuously ultrasonically treat in ethanol for 30 minutes, then continuously ultrasonically treat in deionized water for 30 minutes, and dry to obtain treated PMIA short fibers; immerse the treated PMIA short fibers in a silver ion / DMAC solution (in the silver ion / DMAC solution after immersion, the mass concentration of the treated PMIA short fibers is 11%), the mass ratio between silver ions and the treated PMIA short fibers is 6:1000, and heat at 60 °C for 2 h. ℃ oven for 2 hours, add LiCl (wherein the mass ratio of PMIA to LiCl is 9:6) to the silver ion / DMAC solution, stir continuously at 60 ℃ to obtain a light yellow solution, and finally ultrasonically treat for 1 hour to prepare a PMIA spinning solution, and then use electrospinning to spin the PMIA spinning solution to prepare a silver ion modified nano-aramid film barrier layer, and spin with 2 needles in a horizontal row. The preparation process is as follows: the multi-nozzle electrospinning voltage is 18 kV, the spinning speed is 0.15 ml / h, the distance between the spinning needle and the receiving roller is 16 cm, and the roller speed is 60 min / r;

[0104] (9) immersing the silver ion-modified nano-aramid film barrier layer in a 0.05% sodium borohydride aqueous solution for 30 minutes to reduce the silver ions to nano-silver, and preparing the nano-aramid film barrier layer modified with nano-silver through a reduction reaction, and then immersing it in an ethanol solution for 60 minutes to fully precipitate Li, Cl and other ions;

[0105] (10) Electrostatic spraying (spraying voltage of 11KV, spraying distance of 15cm) is used to coat the nano-silver modified nano-aramid film barrier layer on the surface of the plain weave bearing layer. The thickness of the nano-aramid film barrier layer is about 60 microns, and a multifunctional intelligent protection and danger perception nanofiber fabric can be obtained;

[0106] (11) The multifunctional intelligent protection and hazard perception nanofiber fabric was immersed in a 3% ethanol solution of a fluorinated polymer with a bath ratio of 1:50; then the fabric was taken out and squeezed to dry with a liquid squeeze rate of 40%, steamed for 30 minutes, dried at 70°C for 30 minutes, and finally baked at 110°C for 10 to 30 minutes.

[0107] Example 3

[0108] The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric of this embodiment comprises the following steps:

[0109] (1) 9 g of polyacrylonitrile PAN powder (weight average molecular weight 400,000) was dissolved in 91 g of organic solvent DMF / DMSO solution (DMF / DMSO mass ratio was 9:1), and stirred continuously at room temperature for 24 hours until it was completely dissolved, thereby preparing a spinning solution of polyacrylonitrile PAN;

[0110] (2) adding 0.18 g of tetraethyl orthosilicate to the spinning solution of polyacrylonitrile (PAN), stirring at high speed (100 r / min), to prepare a tetraethyl orthosilicate / PAN composite spinning solution;

[0111] (3) Using an electrospinning machine and an electrospinning process to spin the tetraethyl orthosilicate / PAN composite spinning solution, double nozzle spinning, spinning voltage 15kV; spinning speed 0.2ml / h, the distance between the spinning needle and the bell mouth 12cm; bell mouth speed 100r / min; receiving shaft speed 1.2r / min, to prepare polyacrylonitrile PAN composite yarn;

[0112] (4) Add 0.16 g of silver acetate to 100 ml of 10 mg / ml ethanol solution of titanium carbide multilayer nanosheets (the mass ratio of silver ions to titanium carbide after conversion is 1:10), heat and reflux to adsorb silver ions on the surface and between the layers of titanium carbide, dialyze and dry to obtain silver ion-adsorbed titanium carbide multilayer nanosheets Ag. + @MXene; 2 g of PAN powder and 30 g of tetraethyl orthosilicate were dissolved in 200 g of DMF to obtain a DMF solution of PAN / tetraethyl orthosilicate, and then 1.6 g of Ag was added. + @MXene, high-speed stirring (110r / min stirring), mixed evenly, and obtained Ag + @MXene-doped PAN / ethyl orthosilicate precursor spinning solution; using the PAN / ethyl orthosilicate precursor spinning solution to spray Ag on the surface of the PAN composite yarn through an electrospinning process + @MXene PAN / tetraethyl orthosilicate precursor nanofibers (PAN composite yarn with sprayed Ag + @MXene-doped PAN / TES mass ratio 1:0.8, Ag + @The mass of MXene-doped PAN / ethyl orthosilicate is 80% of the PAN composite yarn), and the electrospinning process is as follows: receiving voltage 18kV, the distance between the needle and the bell mouth is 18cm, the spinning speed is 0.15ml / min; the bell mouth speed is 110r / min; the winding roller speed is 1.5r / min, and the polyacrylonitrile PAN composite core-spun yarn is prepared;

[0113] (5) The polyacrylonitrile (PAN) composite core-spun yarn was drawn by a first-stage drawing multiple of 1.5 times, a second-stage drawing multiple of 0.6 times, and a third-stage drawing multiple of 0.4 times to perform step-by-step drawing and orientation crystallization to improve the mechanical properties; then, it was immersed in an ethanol solution of methyl fumaric acid with a mass fraction of 18%, rolled dry (rolling liquid rate of 60%), dried at 80°C for 30 minutes, and finally baked at 120°C for 10 minutes; finally, a gamma ray radiation source was used as the radiation source. 60 Co was cross-linked by radiation, and the radiation dose was 6×10 -5 rad / s;

[0114] (6) After radiation crosslinking treatment, the polyacrylonitrile PAN core-spun yarn was carbonized at high temperature under nitrogen atmosphere and tension. The carbonization temperature was 800 °C and the tension was 2N. After high temperature carbonization, the polyacrylonitrile PAN composite core-spun yarn was transformed into carbon nanofiber core yarn. Ag + @MXene-doped PAN / TES precursor nanofibers converted to Ag 0 @MXene-doped SiO 2 The nanofibers are wrapped around the outer layer of the carbon nanofiber core yarn. The outer layer of polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofiber to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn, and the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a composite triboelectric nano yarn.

[0115] (7) Weaving the composite triboelectric nano yarn into a plain bearing layer, using the composite triboelectric nano yarn as the warp and weft, the weave structure adopts a 1 / 1 plain weave, the warp density of the fabric is 70 strands / inch, and the weft density is 60 strands / inch;

[0116] (8) Cut PMIA short fibers (length 35 mm-50 mm, diameter 5-30 μm) into pieces (diameter < 0.1 mm), continuously ultrasonically treat in ethanol for 30 minutes, then continuously ultrasonically treat in deionized water for 30 minutes, and dry to obtain treated PMIA short fibers; immerse the treated PMIA short fibers in a silver ion / DMAC solution (in the silver ion / DMAC solution after immersion, the mass concentration of the treated PMIA short fibers is 9%), the mass ratio between silver ions and the treated PMIA short fibers is 6:1000, and heat at 60°C. The mixture was expanded in an oven for 2 hours, LiCl (wherein the mass ratio of PMIA to LiCl was 9:6) was added to the silver ion / DMAC solution, and the mixture was continuously stirred at 60°C to obtain a light yellow solution. The mixture was finally ultrasonically treated for 1 hour to obtain a PMIA spinning solution, and then the PMIA spinning solution was electrospun to prepare a silver ion-modified nano-aramid film barrier layer. Two needles were spun in a horizontal row, and the preparation process was as follows: the multi-nozzle electrospinning voltage was 18 kV, the spinning speed was 0.15 ml / h, the distance between the spinning needle and the receiving roller was 16 cm, and the roller speed was 60 min / r;

[0117] (9) immersing the silver ion-modified nano-aramid film barrier layer in a 0.05% sodium borohydride aqueous solution for 30 minutes to reduce the silver ions to nano-silver, and preparing a nano-aramid film barrier layer modified with nano-silver through a reduction reaction, and then immersing it in an ethanol solution for 60 minutes to fully precipitate Li, Cl and other ions;

[0118] (10) Electrostatic spraying (spraying voltage of 11KV, spraying distance of 15cm) is used to coat the nano-silver modified nano-aramid film barrier layer on the surface of the plain weave bearing layer. The thickness of the nano-aramid film barrier layer is about 60 microns, and a multifunctional intelligent protection and danger perception nanofiber fabric can be obtained;

[0119] (11) The multifunctional intelligent protection and hazard perception nanofiber fabric was immersed in a 3% ethanol solution of a fluorinated polymer with a bath ratio of 1:50; then the fabric was taken out and squeezed to dry with a liquid squeeze rate of 40%, steamed for 30 minutes, dried at 70°C for 30 minutes, and finally baked at 110°C for 20 minutes.

[0120] Example 4

[0121] The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric of this embodiment comprises the following steps:

[0122] (1) 9 g of polyacrylonitrile (PAN) powder (weight average molecular weight 400,000) was dissolved in 91 g of organic solvent DMF / DMSO solution (DMF / DMSO mass ratio was 9:1), and stirred continuously at room temperature for 24 hours until it was completely dissolved, thereby preparing a spinning solution of polyacrylonitrile PAN;

[0123] (2) adding 0.15 g of tetraethyl orthosilicate to the spinning solution of polyacrylonitrile (PAN), stirring at high speed (90 r / min), to prepare a tetraethyl orthosilicate / PAN composite spinning solution;

[0124] (3) Using an electrospinning machine and an electrospinning process to spin the tetraethyl orthosilicate / PAN composite spinning solution, double nozzle spinning, spinning voltage 15kV; spinning speed 0.2ml / h, the distance between the spinning needle and the bell mouth 12cm; bell mouth speed 100r / min; receiving shaft speed 1.2r / min, to prepare polyacrylonitrile PAN composite yarn;

[0125] (4) Add 0.18 g of silver acetate to 100 ml of 10 mg / ml ethanol solution of titanium carbide multilayer nanosheets (the mass ratio of silver ions to titanium carbide after conversion is 1.17:10), heat and reflux to adsorb silver ions on the surface and between the layers of titanium carbide, dialyze and dry to obtain Ag + @MXene; 2 g of PAN powder and 30 g of tetraethyl orthosilicate were dissolved in 200 g of DMF to obtain a DMF solution of PAN / tetraethyl orthosilicate, and then 2.2 g of Ag was added. + @MXene, high-speed stirring (90r / min stirring), mixed evenly, and Ag was prepared + @MXene-doped PAN / ethyl orthosilicate precursor spinning solution; using the PAN / ethyl orthosilicate precursor spinning solution to spray Ag on the surface of the polyacrylonitrile PAN composite yarn through an electrospinning process + @MXene PAN / tetraethyl orthosilicate precursor nanofibers (PAN composite yarn with sprayed Ag + @MXene-doped PAN / TES mass ratio 1:0.65, Ag + @The mass of MXene-doped PAN / ethyl orthosilicate is 65% relative to the PAN composite yarn), and the electrospinning process is as follows: receiving voltage 18kV, the distance between the needle and the bell mouth is 18cm, the spinning speed is 0.15ml / min; the bell mouth speed is 110r / min; the winding roller speed is 1.5r / min, and finally the polyacrylonitrile PAN composite core-spun yarn is prepared;

[0126] (5) The polyacrylonitrile (PAN) composite core-spun yarn was drawn through a first-stage drawing multiple of 1.6 times, a second-stage drawing multiple of 0.6 times, and a third-stage drawing multiple of 0.3 times for step-by-step drawing orientation crystallization to improve the mechanical properties; then, it was immersed in an ethanol solution of maleic acid with a mass fraction of 20%, rolled dry (rolling liquid rate 60%), and then dried at 80°C for 30 minutes, and finally baked at 110°C for 10 minutes; then, a gamma ray radiation source was used as 60 Co was cross-linked by radiation, and the radiation dose was 10×10 -5 rad / s;

[0127] (6) After radiation crosslinking treatment, the polyacrylonitrile PAN core-spun yarn was carbonized at high temperature under nitrogen atmosphere and tension. The carbonization temperature was 800 °C and the tension was 2N. After high temperature carbonization, the polyacrylonitrile PAN composite core-spun yarn was transformed into carbon nanofiber core yarn. Ag + @MXene-doped PAN / TES precursor nanofibers converted to Ag 0 @MXene-doped SiO 2 The nanofibers are wrapped around the outer layer of the carbon nanofiber core yarn. The outer layer of polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofiber to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn; the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a composite triboelectric nano yarn;

[0128] (7) Weaving the composite triboelectric nano yarn into a plain bearing layer, using the composite triboelectric nano yarn as the warp and weft, the weave structure adopts 1 / 1 plain weave, the warp density of the fabric is 70 strands / inch, and the weft density is 60 strands / inch;

[0129] (8) PMIA short fibers (length 35 mm-50 mm, diameter 5-30 μm) were cut into pieces (diameter < 0.1 mm), and the pieces were continuously ultrasonically treated in ethanol for 30 minutes, and then continuously ultrasonically treated in deionized water for 30 minutes, and dried to obtain treated PMIA short fibers; the treated PMIA short fibers were immersed in a silver ion / DMAC solution (the mass concentration of the treated PMIA short fibers in the silver ion / DMAC solution after immersion was 10%), the mass ratio of silver ions to PMIA short fibers was 6:1000, and the mixture was heated at 60°C. The mixture was expanded in an oven for 2 hours, and then LiCl (wherein the mass ratio of PMIA to LiCl was 9:6) was added to the silver ion / DMAC solution, and the mixture was continuously stirred at 60°C to obtain a light yellow solution. Finally, the mixture was ultrasonically treated for 1 hour to prepare a PMIA spinning solution, and then the PMIA spinning solution was electrospun to prepare a silver ion-modified nano-aramid film barrier layer, and two needles were spun in a horizontal row. The preparation process was as follows: the multi-nozzle electrospinning voltage was 18 kV, the spinning speed was 0.15 ml / h, the spinning needle was 16 cm away from the receiving roller, and the roller speed was 60 min / r;

[0130] (9) immersing the silver ion-modified nano-aramid film barrier layer in a 0.05% sodium borohydride aqueous solution for 30 minutes to reduce the silver ions to nano-silver, and preparing a nano-aramid film barrier layer modified with nano-silver through a reduction reaction, and then immersing it in an ethanol solution for 60 minutes to fully precipitate Li, Cl and other ions;

[0131] (10) Electrostatic spraying (spraying voltage of 11KV, spraying distance of 15cm) is used to coat the nano-silver modified nano-aramid film barrier layer on the surface of the plain weave bearing layer. The thickness of the nano-aramid film barrier layer is about 60 microns, and a multifunctional intelligent protection and danger perception nanofiber fabric can be obtained;

[0132] (11) The multifunctional intelligent protection and hazard perception nanofiber fabric was immersed in a 3% ethanol solution of a fluorinated polymer with a bath ratio of 1:50; then the fabric was taken out and squeezed to dry with a liquid squeeze rate of 40%, steam fumigated for 30 minutes, dried at 70°C for 30 minutes, and finally baked at 110°C for 25 minutes.

[0133] Example 5

[0134] The wireless sensing transmission system of this embodiment includes the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 and a wireless signal collector. The wireless signal collector has 32 channels and can be connected to 32 pieces of prepared intelligent fabrics at the same time to collect electrical signals from different positions of the human body. In this embodiment, two pieces of fabric TENG1 and TENG2 made of the multifunctional intelligent protection and danger perception nanofiber fabric in Example 1 are integrated into the abdomen of the clothing for remote information exchange.

[0135] The prepared smart textile (i.e., the multifunctional smart protection and danger perception nanofiber fabric prepared in Example 1) and a wireless data acquisition card (power supply required) are used to form a wireless smart danger perception system, such as Figure 3 As shown in (a); the corresponding intelligent hazard perception system is integrated into the chemical protective clothing. The hands continuously tap the intelligent fabric, and the computer can receive the corresponding signal through wireless WIFI, thereby realizing the perception of dangerous environment, such as Figure 3 (b) as shown.

[0136] Experimental Example 1 Contact and Separation Friction Experiment

[0137] The multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 was subjected to a contact separation friction test using a numerically controlled contact pressure device. The contact frequency was set to 2 Hz and the contact pressure was set to 30N.

[0138] Voltage, current and electric power are important indicators to characterize the stability and durability of the piezoelectric properties of fabrics. Figure 2 (a) and Figure 2 (b) The test voltage and current results of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 with a size of 2.5 cm*2 cm. Figure 2 (a) and Figure 2 (b) It can be seen that the voltage of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 can reach 23V and the current can reach 230nA, so the electric power can be calculated to be 10.58mW / m 2 After 3000 times of touch and pressure, the induced voltage increased slightly, indicating that the triboelectric properties of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 have high durability and stability. The voltage of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Examples 2-4 can reach 20.8V, and the current can reach 218nA, so the electric power can be calculated to be 9.07mW / m 2 .

[0139] Experimental Example 2 Flame retardant test

[0140] The flame retardant test was carried out according to the vertical combustion method, and the experimental process was carried out in accordance with the "Standard Test Method for Fire Resistance of Textiles (Vertical Test)".

[0141] The experimental results show that the flame retardant properties of the multifunctional intelligent protection and hazard perception nanofiber fabrics prepared in Examples 1-4 all reach the V0 level.

[0142] Experimental Example 3: Acid and alkali resistance test

[0143] The multifunctional intelligent protective and hazard-sensing nanofiber fabric prepared in Example 1 was tested for liquid repellency according to the standard GB24539-2021 Protective Clothing Chemical Protective Clothing. The test results are as follows: Figure 5 As shown, it can be known that the liquid repellency of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 to 30% sodium hydroxide, 40% nitric acid, and 80% sulfuric acid solutions is greater than 97%, indicating that it has good acid and alkali resistance.

[0144] Experimental Example 4: High temperature fire scene perception experiment

[0145] The multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 was woven into a finished product with an area of ​​0.5 cm*0.5 cm to 1 cm*1 cm, which was integrated into the elbow or abdomen. The test results were as follows: Figure 7 (a) and Figure 7 As shown in (b), it can be seen that when entering the fire environment, the elbow bending voltage signal increases by 137% (see Figure 7 (a)), the sensing signal of hand-patting fabric increases by more than 9 times (see Figure 7 (b)), indicating that it can sense high-temperature fire scenes.

[0146] Experimental Example 5: Strong Acid and Strong Alkali Perception Experiment

[0147] The multifunctional intelligent protection and danger sensing nanofiber fabric prepared in Example 1 was vertically contacted with the surface of a strong acid and alkali solution (30% sodium hydroxide solution, 80% sulfuric acid solution) at a contact frequency of 1.5 Hz to test the induced voltage generated after the fabric was contacted with the solution. The test results are shown in Figure 2. Figure 6 As shown, it can be seen that the voltage generated after contacting 30% sodium hydroxide is >16.5V, and the voltage generated after contacting 80% sulfuric acid solution is ~8V, indicating that it has the ability to recognize strong acids and bases.

[0148] Experimental Example 6 Antibacterial Experiment

[0149] The multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 was tested according to the standard of "GB / T20944.3-2008 Part 3 Oscillation Method".

[0150] Test results such as Figure 4As shown, no colonies appeared in the four areas of the culture dish, indicating that the antibacterial rates of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 against Escherichia coli and Staphylococcus aureus reached 99.999% and 99.99%, respectively, which indicates that it has antibacterial properties.

[0151] Experimental Example 7 Antiviral Experiment

[0152] The multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 was tested by the Guangdong Microbiological Analysis and Testing Center using the ISO18184:2019 (E) "Testing the Antiviral Activity of Textiles" method. The test results showed that the antiviral inactivation rate of the multifunctional intelligent protection and danger perception nanofiber fabric prepared in Example 1 against H3N2 reached 99.42%, indicating that it has strong antiviral ability.

[0153] Experimental Example 8 Hydrostatic Pressure Resistance and Moisture Permeability Test

[0154] The hydrostatic pressure resistance was tested using the national standard method GB / T 4744-2013 "Hydrostatic pressure method for testing and evaluating the waterproof performance of textiles", and the moisture permeability was tested using the national standard test method GB / T 12704.2-2009 "Textiles. Test method for moisture permeability of fabrics. Part 2: Evaporation method", which was conducted by the Jiangsu Textile Product Quality Supervision and Inspection Institute. The test results show that the hydrostatic pressure resistance of the multifunctional intelligent protection and hazard perception nanofiber fabric prepared in Example 1 is 8780 mmH 2 O; The moisture permeability test result is >8000g / (m 2 ·D).

[0155] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A multifunctional intelligent protection and danger sensing nanofiber fabric, It is characterized in that It includes: A plain bearing layer and a nano-aramid film barrier layer coated on the surface of the plain bearing layer; wherein the plain bearing layer is woven from a composite triboelectric nano yarn, and the composite triboelectric nano yarn comprises a carbon nanofiber core yarn and Ag wrapped around the outer layer of the carbon nanofiber core yarn. 0 @Mxene-doped SiO 2 Nanofibers.

2. A method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 1, It is characterized in that The following steps are involved: Preparation of alkyl silicate / polyacrylonitrile (PAN) composite spinning solution; Spinning the alkyl silicate / polyacrylonitrile (PAN) composite spinning solution into yarn to prepare polyacrylonitrile (PAN) composite yarn; Preparation of Ag + @MXene doped PAN / alkyl silicate precursor spinning solution, using the PAN / alkyl orthosilicate precursor spinning solution, spraying the Ag on the surface of the polyacrylonitrile PAN composite yarn + @MXene-doped polyacrylonitrile PAN / alkyl silicate precursor nanofibers to prepare polyacrylonitrile PAN composite core-spun yarn; The polyacrylonitrile (PAN) composite core-spun yarn is immersed in a forming agent solution, and then subjected to radiation cross-linking treatment; The polyacrylonitrile (PAN) composite core-spun yarn after radiation cross-linking was carbonized to prepare the composite triboelectric nano yarn. Weaving the composite triboelectric nano yarn into a plain weave load-bearing layer; preparing a PMIA spinning solution, and then weaving the PMIA spinning solution into a silver ion-modified nano-aramid film barrier layer; The silver ion modified nano-aramid film barrier layer is subjected to a reduction reaction to obtain a nano-silver modified nano-aramid film barrier layer; The nano-silver modified nano-aramid film barrier layer is coated on the surface of the plain weave bearing layer to obtain the barrier layer.

3. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 2, It is characterized in that The following steps are involved: S1, adding ultra-high molecular weight polyacrylonitrile PAN into a polar aprotic solvent to prepare a spinning solution of polyacrylonitrile PAN; S2, adding alkyl silicate to the spinning solution of polyacrylonitrile PAN to prepare alkyl silicate / polyacrylonitrile PAN composite spinning solution; S3, spinning the alkyl silicate / polyacrylonitrile (PAN) composite spinning solution into yarn using an electrostatic spinning process to prepare polyacrylonitrile (PAN) composite yarn; S4, adding soluble silver salt to the titanium carbide multilayer nanosheet solution, heating and refluxing to adsorb silver ions on the surface and between the layers of titanium carbide, and preparing silver ion adsorbed titanium carbide multilayer nanosheets Ag + @MXene; Ultra-high molecular weight polyacrylonitrile PAN and alkyl silicate are dissolved in a polar aprotic solvent, and then silver ion-adsorbed titanium carbide multilayer nanosheets Ag are added + @MXene, prepared Ag + @MXene-doped PAN / alkyl silicate precursor spinning solution; using the PAN / ethyl orthosilicate precursor spinning solution to spray the Ag on the surface of the polyacrylonitrile PAN composite yarn through an electrospinning process + @MXene-doped polyacrylonitrile PAN / alkyl silicate precursor nanofibers were used to prepare polyacrylonitrile PAN composite core-spun yarn; S5, the polyacrylonitrile (PAN) composite core-spun yarn is drawn step by step, immersed in a forming agent solution, rolled dry, dried, and finally baked (for example, rolled dry (liquid rolling rate 30-80%, preferably 60%), then dried at 60-100° C. for 10-60 min, and finally baked at 100-130° C., preferably 110-120° C. for 5-30 min), and then cross-linked by gamma ray radiation; S6, the polyacrylonitrile PAN composite core-spun yarn after radiation cross-linking treatment is carbonized, and the polyacrylonitrile PAN composite core-spun yarn is transformed into carbon nanofiber core yarn after carbonization. + Conversion of MXene-doped polyacrylonitrile PAN / alkyl silicate precursor nanofibers into Ag 0 @Mxene-doped SiO 2 The nanofibers are wrapped in the outer layer of the carbon nano core yarn, and the polyacrylonitrile PAN component is converted into a carbon structure and connected to the core carbon nanofibers to form a conductive path, ensuring that SiO 2 The triboelectric signal is quickly transferred to the carbon nanofiber core yarn; the silver ions adsorbed by MXene are reduced to elemental silver by carbon monoxide, thereby preparing a composite triboelectric nano yarn; S7, weaving the composite triboelectric nano yarn into a plain weave load-bearing layer; S8, preparing a PMIA spinning solution, and then using the PMIA spinning solution to prepare a silver ion-modified nano-aramid film barrier layer by an electrospinning process; S9, the silver ion modified nano-aramid film barrier layer is subjected to a reduction reaction to obtain a nano-silver modified nano-aramid film barrier layer; S10. The nano-silver modified nano-aramid film barrier layer is coated on the surface of the plain weave bearing layer by electrostatic spraying to obtain a multifunctional intelligent protection and danger perception nanofiber fabric.

4. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 3, It is characterized in that In step S1, the molecular weight of the ultra-high molecular weight polyacrylonitrile is 300,000-700,000, preferably 400,000-500,000, and is preferably prepared by gamma ray in-situ irradiation polymerization; and / or, In step S1, the polar aprotic solvent is selected from at least one of dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and sulfolane, preferably a mixed solution of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), preferably, the mass ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is 15:1 to 8:1, preferably 12 to 8:1, more preferably 10 to 9:1; and / or, In step S1, the mass concentration of ultra-high molecular weight polyacrylonitrile in the spinning solution of polyacrylonitrile PAN is 5-18%, preferably 7-15%, and more preferably 8-12%.

5. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 3, It is characterized in that In step S2, the alkyl silicate is selected from at least one of ethyl orthosilicate, methyl orthosilicate and butyl orthosilicate, preferably ethyl orthosilicate; and / or, In step S2, the amount of alkyl silicate such as ethyl orthosilicate added is 0.2-5% of the mass of ultra-high molecular weight polyacrylonitrile, preferably 1-3%, more preferably 1.5-2%; and / or, In step S3, in the electrospinning process, the double-nozzle electrospinning voltage is 5-20 kV, preferably 8-15 kV; the spinning speed is 0.01-0.5 ml / h, preferably 0.08-0.22 ml / h; the distance between the spinning needle and the bell mouth is 10-15 cm; the bell mouth speed is 50-150 r / min, preferably 80-130 r / min, more preferably 85-125 r / min; the receiving shaft speed is 0.01-5 r / min, preferably 0.1-3 r / min, more preferably 0.2-3 r / min.

6. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 3, It is characterized in that In step S4, the soluble silver salt is selected from at least one of silver acetate and silver tartrate, preferably silver acetate; and / or, In step S4, the mass ratio of the soluble silver salt to the titanium carbide multilayer nanosheets is 0.1:10 to 3:10, preferably 1:10, calculated as silver ions; and / or In step S4, the alkyl silicate is selected from at least one of ethyl orthosilicate, methyl orthosilicate and butyl orthosilicate, preferably ethyl orthosilicate; and / or, In step S4, the mass ratio of ultra-high molecular weight polyacrylonitrile PAN to alkyl silicate is 1:5 to 1:30, preferably 1:10 to 1:20, more preferably 1:15; and / or, In step S4, the polar aprotic solvent is selected from at least one of dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and sulfolane, preferably dimethylformamide (DMF); and / or, In step S4, the mass ratio of PAN / alkyl silicate to the polar aprotic solvent is 10-25%:1; and / or, In step S4, the silver ion adsorbed titanium carbide multilayer nanosheet Ag + The mass ratio of @MXene to PAN / alkyl silicate is 1-30%:1, preferably 4-25%:1, preferably 5-20%:1, preferably 8-15%:1; and / or, In step S4, in the electrospinning process, the receiving voltage is 10-50 kV, preferably 15-35 kV, the distance between the needle and the bell mouth is 10-25 cm, preferably 16-22 cm, the spinning speed is 0.05 ml / min-0.3 ml / min, preferably 0.10 ml / min-0.20 ml / min; the bell mouth speed is 70 r / min-150 r / min, preferably 90-130 r / min; the winding roller speed is 0.1 r / min-5 r / min, preferably 0.15-2.6 r / min.

7. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 3, It is characterized in that In step S5, the polyacrylonitrile (PAN) composite core-spun yarn is subjected to three-stage drafting, wherein the first-stage drafting multiple is 1.5 to 1.8, the second-stage drafting multiple is 0.5 to 1.2, and the third-stage drafting multiple is 0.3 to 0.5; and / or, In step S5, the molding agent is selected from at least one of crotonic acid, maleic acid, and methyl fumaric acid, preferably maleic acid or methyl fumaric acid, more preferably an ethanol solution of maleic acid with a mass fraction of 20% or an ethanol solution of methyl fumaric acid with a mass fraction of 18%; and / or, In step S5, the radiation source of the gamma ray radiation cross-linking treatment is 60 Co, radiation dose is 5~13×10 -5 rad / s; and / or, In step S6, high temperature carbonization is performed in a nitrogen atmosphere under tension, wherein the carbonization temperature of the high temperature carbonization is 600-1500° C., preferably 600-1000° C., more preferably 800° C.; the tension is 0.1-30N, preferably 0.8-2.6N; and / or, In step S7, the composite triboelectric nano yarn is warp yarn and weft yarn, the weave structure is 1 / 1 plain weave, the warp density of the fabric is 20 to 150 strands / inch, preferably 30 to 78 strands / inch; the weft density is 10 to 70 strands / inch, preferably 20 to 68 strands / inch.

8. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to claim 3, It is characterized in that In step S8, the PMIA spinning solution is prepared according to the following method: PMIA staple fibers are cut into pieces, ultrasonically treated in ethanol (e.g., ultrasonically treated for 10 to 60 minutes, preferably 20 to 40 minutes), and then ultrasonically treated in deionized water (e.g., ultrasonically treated for 10 to 60 minutes, preferably 20 to 40 minutes), and dried to obtain treated PMIA staple fibers; the treated PMIA staple fibers are immersed in a silver ion / DMAC solution, wherein the mass concentration of the treated PMIA staple fibers in the silver ion / DMAC solution after immersion is 6% to 15%, and the silver ion / DMAC solution after immersion is 10% to 20%. The mass ratio of the silver ion to the treated PMIA staple fibers is 2:1000 to 10:1000, preferably 4:1000 to 8:1000, and the silver ion / DMAC solution is expanded at 30-80°C, preferably 60°C, for 0.5-5 hours, preferably 2 hours, and then LiCl is added to the silver ion / DMAC solution (the mass ratio of PMIA to LiCl is (5-15): (1-10), preferably 9:6), stirred at 30-80°C, preferably 60°C, and finally ultrasonically treated (for example, ultrasonically treated for 0.5 to 2 hours, preferably 1 hour) to obtain a PMIA spinning solution; and / or, In step S8, in the electrospinning process, the spinning voltage is 5 to 50 kV, preferably 12 to 20 kV; the spinning speed is 0.01 to 0.3 ml / h, preferably 0.05 to 0.2 ml / h; the distance between the spinning needle and the receiving roller is 10 to 30 cm, preferably 15 to 25 cm; the roller speed is 10 to 150 r / min, preferably 30 to 90 r / min; and / or, In step S9, the silver ion modified nano-aramid film barrier layer is immersed in an aqueous solution of sodium borohydride with a mass concentration of 0.01% to 1% for 10-150 minutes, preferably 30 to 120 minutes, to reduce the silver ions to nano-silver, to prepare a nano-aramid film barrier layer modified with nano-silver, and then immersed in an ethanol solution and fully immersed for 20-80 minutes, preferably 40 to 60 minutes.

9. The method for preparing the multifunctional intelligent protection and danger perception nanofiber fabric according to any one of claims 3 to 8, It is characterized in that After step S10, the following step is also included: surface hydrophobic treatment of the multifunctional intelligent protection and danger perception nanofiber fabric: S11, immersing the multifunctional intelligent protection and danger perception nanofiber fabric in an ethanol solution of a fluorine-containing finishing agent (for example, the mass concentration of the fluorine-containing finishing agent in the ethanol solution of the fluorine-containing finishing agent is 1-15%, preferably 1-5%, and more preferably 1-3%), with a bath ratio of 1:30-1:100, preferably 1:50; then taking out and rolling dry, with a rolling rate of 10-90%, preferably 20%-40%; steam fumigation treatment for 10-60min, preferably 30min, and then drying at 60-80℃ for 20-50min, and finally baking at 110-140℃ for 10-30min.

10. A wireless sensor transmission system, It is characterized in that It comprises the multifunctional intelligent protection and danger perception nanofiber fabric as described in claim 1 or the multifunctional intelligent protection and danger perception nanofiber fabric prepared by the preparation method described in any one of claims 2-9.

Citation Information

Patent Citations

  • In-situ polymerized surface modified fiber-based friction nano-generator and preparation thereof

    CN108667339A

  • Knitted flexible sensing fabric based on Mxene coated conductive yarn and preparation method

    CN112251897A

  • Preparation method of silver nanowire-MXene super-elastic intelligent conductive fiber

    CN113322667A

  • Flexible high-strength silicon dioxide nanofiber membrane and preparation method thereof

    CN113944008A

  • Preparation and application of conductive aramid nanofiber membrane

    CN114892395A