Preparation method of porous heat-insulating film and automobile film applying porous heat-insulating film

The porous thermal insulation film prepared by electrospinning solves the problem of poor thermal insulation effect of existing sunscreen films under extreme high temperatures, and achieves efficient barriers of infrared and ultraviolet rays, significantly cools down, and remains stable in extreme climates. Environmentally friendly and easy to recycle.

CN119041099AActive Publication Date: 2024-11-29ZHEJIANG ROUHE NEW ENERGY MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411113694.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing sunscreen film cannot effectively block the indoor temperature rise in extreme high temperature weather, and has poor quality and short life, so it cannot completely block ultraviolet rays, affecting the sunscreen effect and beauty.

Method used

By preparing PVDF-b-PTFE powder and mixing it with barium titanate nanoparticles, a porous thermal insulation film was prepared by electrospinning process to form a BTO/PVDF-b-PTFE nanofiber thermal insulation film, with high porosity and soft bending resistance. Folding characteristics.

Benefits of technology

This porous heat insulation film can effectively block infrared and ultraviolet rays for a long time, significantly reduce indoor and vehicle temperatures, high reflectivity and high emissivity, and can cool down by 10-80℃ after coverage, and remains stable in extreme climates. The material is environmentally friendly and easy to recycle. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a porous heat-insulating film. The preparation method comprises the following steps: step 1, preparing PVDF-b-PTFE powder; step 2, adding the PVDF-b-PTFE powder obtained in the step 1 into a mixed solution of N, N-dimethylformamide and acetone, so as to obtain a precursor spinning solution; step 3, adding barium titanate nanoparticles into the precursor spinning solution obtained in the step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; step 4, performing spinning processing on the BTO / PVDF-b-PTFE mixed solution obtained in the step 3 through an electrostatic spinning process to obtain a porous heat-insulating film; the porous heat insulation film prepared through electrostatic spinning is a BTO / PVDF-b-PTFE nanofiber heat insulation film, has good durability, can effectively block infrared rays and ultraviolet rays for a long time, and remarkably reduces the indoor temperature and the in-vehicle temperature. In the manufacturing and using processes, harmful substances are not released, the raw materials are relatively easy to recycle and treat, and the material is an environment-friendly material with an energy-saving effect, can be kept stable under an extreme weather condition, and has relatively high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal insulation film preparation, and in particular to a method for preparing a porous thermal insulation film and an automobile film using the porous thermal insulation film. Background Art

[0002] The solar spectrum covers three main bands: the first is the ultraviolet band of 200-400nm, which accounts for 3% of the sunlight energy; the second is the visible light band of 400-760nm, which accounts for 44%; and the last is the infrared band of 760-2500nm, which accounts for 53% of the energy, becoming the most significant part of sunlight. In the hot summer, the sunlight is particularly strong. When the sunlight enters the room or car through the glass, the temperature will rise sharply, greatly affecting the living environment and the riding experience. Among them, the infrared band has become the main factor causing the temperature to rise at the irradiation point due to its huge energy share. At present, it mainly relies on glass film to block infrared rays to reduce the sharp rise in temperature inside the car. However, the existing sun-proof and heat-insulating films have limited insulation effects. They can only block a portion of infrared rays, but cannot block ultraviolet rays, and the insulation effect is not significant. Especially in extremely hot weather, the film may not be able to completely prevent the indoor temperature from rising. In addition, the film has poor quality and a short lifespan. After long-term use, it will experience problems such as aging, bubbling, and falling off, which will not only affect its sun-proof and heat-insulating effects, but may also affect its appearance. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a porous heat-insulating film which is reliable in use, has good heat-insulating effect and can prevent ultraviolet rays, and an automobile film using the porous heat-insulating film.

[0004] In order to solve the above technical problems, the present invention is solved by the following technical solutions: A method for preparing a porous thermal insulation film, comprising: Step 1, preparing PVDF-b-PTFE powder; Step 2: adding the PVDF-b-PTFE powder obtained in step 1 to an N,N-dimethylformamide solution, or a mixture of N,N-dimethylformamide and acetone to obtain a precursor spinning solution; Step 3: adding barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation membrane.

[0005] Preferably, the preparation process of PVDF-b-PTFE powder in step 1 is: A1. Add deionized water into the reactor and heat the reactor; A2, adding initiator to the reactor and mixing evenly with a stirrer; A3, adding vinylidene fluoride monomer gas into the reactor, and introducing tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 15-25%, stop the reaction and remove the latex-like PVDF-b-PTFE; A5. The latex-like PVDF-b-PTFE obtained above is naturally dried, and after drying, it is ground by a ball mill to obtain PVDF-b-PTFE powder.

[0006] Furthermore, the reactor is a 40-liter reactor; the weight of deionized water is 22.5 kilograms; the heating temperature of the reactor in step A1 is 80°C and maintained; the initiator added to the reactor is 100 to 200 grams; in step A3, vinylidene fluoride monomer gas is added to the reactor so that the pressure in the reactor reaches 0.35 MPa; and then tetrafluoroethylene monomer gas is introduced until the pressure in the reactor reaches 1.52 MPa.

[0007] Furthermore, the initiator is a nitroxide free radical initiator.

[0008] On the basis of the above, the nitroxide free radical initiator includes: one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butylbenzene peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

[0009] Furthermore, in step A3, the weight ratio of the vinylidene fluoride monomer gas to the tetrafluoroethylene monomer gas introduced into the reactor is 0.8-1.2:1.

[0010] Preferably, the preparation process of the precursor spinning solution in step 2 is: adding PVDF-b-PTFE powder to a mixed solvent of N,N-dimethylformamide and acetone, and stirring for 2-6 hours in a water bath at 50-80°C; wherein the volume ratio of N,N-dimethylformamide to acetone is 1:0-10.

[0011] Preferably, the preparation process of the BTO / PVDF-b-PTFE mixed solution in step three is: mixing barium titanate nanoparticles with a precursor spinning solution, and stirring for 6 to 12 hours in a water bath at 40 to 70°C; wherein the mass ratio of the barium titanate nanoparticles to the precursor spinning solution is 1:2 to 10.

[0012] Preferably, in step 4, the electrostatic voltage of electrospinning is 20-80 kV, the receiving distance is 10-60 cm, the perfusion rate is 20-1500 mL / h, the spinning temperature is 25-40° C., and the relative humidity is 35%-65%.

[0013] An automotive film using a porous thermal insulation film prepared by the porous thermal insulation film preparation method of claim 1, characterized in that it comprises at least one layer of porous thermal insulation film.

[0014] Compared with the prior art, the present invention has the following beneficial effects: the porous thermal insulation film prepared by electrospinning is a BTO / PVDF-b-PTFE nanofiber thermal insulation film with good durability, which can effectively block infrared and ultraviolet rays for a long time, and significantly reduce the indoor and in-car temperature. The high sunlight reflectivity is as high as 80-99.8% and the high and medium infrared emissivity is as high as 70-99.8%. The interior temperature of the car covered with the porous BTO / PVDF-b-PTFE thermal insulation film can be reduced by more than 5-55°C compared with the commercial vehicle cover, and can be reduced by more than 10-80°C compared with the model without fabric covering.

[0015] The present invention does not release harmful substances during the manufacturing and use processes, and the raw materials are relatively easy to recycle and process. It is an environmentally friendly material that can have energy-saving effects. At the same time, it can remain stable under extreme climatic conditions and has strong stability.

[0016] The heat-insulating film prepared by electrospinning in the present invention is a nanofiber film, which has excellent properties such as high porosity, softness, bending resistance, and stretchability. The porosity of the material is 60-80%, the thickness is 0.1-10mm, and the fiber diameter is 50-1000nm. DETAILED DESCRIPTION

[0017] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be used for other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0018] Embodiment 1: A method for preparing a porous thermal insulation film, comprising: Step 1, prepare PVDF-b-PTFE powder; the preparation process of PVDF-b-PTFE powder is as follows: A1, add deionized water to the reactor, and heat the reactor; A2, add an initiator to the reactor and mix evenly with an agitator; A3, add vinylidene fluoride monomer gas to the reactor, and introduce tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 15%, stop the reaction and remove the latex PVDF-b-PTFE; A5, naturally dry the latex PVDF-b-PTFE obtained above, and grind it with a ball mill after drying to obtain PVDF-b-PTFE powder.

[0019] Specifically, 22.5 kg of deionized water is added to a 40-liter reactor, and the reactor is heated to 80°C, 100 g of initiator is added, and the stirrer speed is set to 200 rpm to ensure that the reaction is evenly mixed; vinylidene fluoride monomer gas is added to the reactor to make the pressure in the reactor reach 0.35 MPa, and then tetrafluoroethylene monomer gas is introduced to increase the pressure of the reactor until the pressure in the reactor reaches 1.52 MPa; during this period, an additional 2500 g of deionized water can be added to accelerate the dissolution and continue the reaction until the solid content reaches 15%, the reaction is stopped, and the latex is discharged from the reactor, and after natural drying, it is put into a ball mill for grinding to form PVDF-b-PTFE powder. The weight ratio of the vinylidene fluoride monomer gas and the tetrafluoroethylene monomer gas introduced into the reactor is 0.8:1.

[0020] The above-mentioned initiator is a nitroxide free radical initiator, specifically one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butylbenzene peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

[0021] Step 2: Add the PVDF-b-PTFE powder obtained in step 1 to a mixed solution of N, N-dimethylformamide and acetone to obtain a precursor spinning solution; specifically, the preparation process of the precursor spinning solution is: add the PVDF-b-PTFE powder to a mixed solvent of N, N-dimethylformamide and acetone, and stir for 6 hours under a 50°C water bath condition; wherein the volume ratio of N, N-dimethylformamide to acetone is 1:10. The configured acetone can accelerate dissolution.

[0022] Step 3: Add barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; specifically, the preparation process of the BTO / PVDF-b-PTFE mixed solution is: mix the barium titanate nanoparticles with the precursor spinning solution, and stir for 12 hours in a 40°C water bath; wherein the mass ratio of the barium titanate nanoparticles to the precursor spinning solution is 1:2.

[0023] Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation film, wherein the electrostatic voltage of the electrospinning is 20 kV, the receiving distance is 10 cm, the perfusion rate is 20 mL / h, the spinning temperature is 25° C., and the relative humidity is 65%.

[0024] Embodiment 2: A method for preparing a porous thermal insulation film, comprising: Step 1, prepare PVDF-b-PTFE powder; the preparation process of PVDF-b-PTFE powder is as follows: A1, add deionized water to the reactor, and heat the reactor; A2, add an initiator to the reactor and mix evenly with an agitator; A3, add vinylidene fluoride monomer gas to the reactor, and introduce tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 25%, stop the reaction and remove the latex PVDF-b-PTFE; A5, naturally dry the latex PVDF-b-PTFE obtained above, and grind it with a ball mill after drying to obtain PVDF-b-PTFE powder.

[0025] Specifically, 22.5 kg of deionized water is added to a 40-liter reactor, and the reactor is heated to 80°C, 200 g of initiator is added, and the stirrer speed is set to 400 rpm to ensure that the reaction is evenly mixed; vinylidene fluoride monomer gas is added to the reactor to make the pressure in the reactor reach 0.35 MPa, and then tetrafluoroethylene monomer gas is introduced to increase the pressure of the reactor until the pressure in the reactor reaches 1.52 MPa; during this period, an additional 2500 g of deionized water can be added to accelerate the dissolution and continue the reaction until the solid content reaches 25%, the reaction is stopped, and the latex is discharged from the reactor, and after natural drying, it is put into a ball mill for grinding to form PVDF-b-PTFE powder. The weight ratio of the vinylidene fluoride monomer gas and the tetrafluoroethylene monomer gas introduced into the reactor is 1.2:1.

[0026] The above-mentioned initiator is a nitroxide free radical initiator, specifically one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butylbenzene peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

[0027] Step 2: Add the PVDF-b-PTFE powder obtained in step 1 to a mixed solution of N,N-dimethylformamide and acetone to obtain a precursor spinning solution; specifically, the preparation process of the precursor spinning solution is: add the PVDF-b-PTFE powder to a mixed solvent of N,N-dimethylformamide and acetone, and stir for 2 hours in a water bath at 80°C; wherein the volume ratio of N,N-dimethylformamide to acetone is 1:5.

[0028] Step 3: Add barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; specifically, the preparation process of the BTO / PVDF-b-PTFE mixed solution is: mix the barium titanate nanoparticles with the precursor spinning solution, and stir for 6 hours in a 70°C water bath; wherein the mass ratio of the barium titanate nanoparticles to the precursor spinning solution is 1:10.

[0029] Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation film, wherein the electrostatic voltage of the electrospinning is 80 kV, the receiving distance is 60 cm, the perfusion rate is 1500 mL / h, the spinning temperature is 40° C., and the relative humidity is 35%.

[0030] Embodiment 3: A method for preparing a porous thermal insulation film, comprising: Step 1, prepare PVDF-b-PTFE powder; the preparation process of PVDF-b-PTFE powder is as follows: A1, add deionized water to the reactor, and heat the reactor; A2, add an initiator to the reactor and mix evenly with an agitator; A3, add vinylidene fluoride monomer gas to the reactor, and introduce tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 20%, stop the reaction and remove the latex PVDF-b-PTFE; A5, naturally dry the latex PVDF-b-PTFE obtained above, and grind it with a ball mill after drying to obtain PVDF-b-PTFE powder.

[0031] Specifically, 22.5 kg of deionized water is added to a 40-liter reactor, and the reactor is heated to 80°C, 150 g of initiator is added, and the stirrer speed is set to 300 rpm to ensure that the reaction is evenly mixed; vinylidene fluoride monomer gas is added to the reactor to make the pressure in the reactor reach 0.35 MPa, and then tetrafluoroethylene monomer gas is introduced to increase the pressure of the reactor until the pressure in the reactor reaches 1.52 MPa; during this period, an additional 2500 g of deionized water can be added to accelerate the dissolution and continue the reaction until the solid content reaches 20%, the reaction is stopped, and the latex is discharged from the reactor, and after natural drying, it is put into a ball mill for grinding to form PVDF-b-PTFE powder. The weight ratio of the vinylidene fluoride monomer gas and the tetrafluoroethylene monomer gas introduced into the reactor is 1:1.

[0032] The above-mentioned initiator is a nitroxide free radical initiator, specifically one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butylbenzene peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

[0033] Step 2: Add the PVDF-b-PTFE powder obtained in step 1 to a mixed solution of N,N-dimethylformamide and acetone to obtain a precursor spinning solution; specifically, the preparation process of the precursor spinning solution is: add the PVDF-b-PTFE powder to a mixed solvent of N,N-dimethylformamide and acetone, and stir for 4 hours in a water bath at 60°C; wherein the volume ratio of N,N-dimethylformamide to acetone is 1:1.

[0034] Step 3: Add barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; specifically, the preparation process of the BTO / PVDF-b-PTFE mixed solution is: mix the barium titanate nanoparticles with the precursor spinning solution, and stir for 8 hours in a 50°C water bath; wherein the mass ratio of the barium titanate nanoparticles to the precursor spinning solution is 1:6.

[0035] Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation film, wherein the electrostatic voltage of the electrospinning is 50 kV, the receiving distance is 40 cm, the perfusion rate is 700 mL / h, the spinning temperature is 35° C., and the relative humidity is 50%.

[0036] Embodiment 4: A method for preparing a porous thermal insulation film, comprising: Step 1, prepare PVDF-b-PTFE powder; the preparation process of PVDF-b-PTFE powder is as follows: A1, add deionized water to the reactor, and heat the reactor; A2, add an initiator to the reactor and mix evenly with an agitator; A3, add vinylidene fluoride monomer gas to the reactor, and introduce tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 20%, stop the reaction and remove the latex PVDF-b-PTFE; A5, naturally dry the latex PVDF-b-PTFE obtained above, and grind it with a ball mill after drying to obtain PVDF-b-PTFE powder.

[0037] Specifically, 22.5 kg of deionized water is added to a 40-liter reactor, and the reactor is heated to 80°C, 200 g of initiator is added, and the stirrer speed is set to 400 rpm to ensure that the reaction is evenly mixed; vinylidene fluoride monomer gas is added to the reactor to make the pressure in the reactor reach 0.35 MPa, and then tetrafluoroethylene monomer gas is introduced to increase the pressure of the reactor until the pressure in the reactor reaches 1.52 MPa; during this period, an additional 2500 g of deionized water can be added to accelerate the dissolution and continue the reaction until the solid content reaches 20%, the reaction is stopped, and the latex is discharged from the reactor, and after natural drying, it is put into a ball mill for grinding to form PVDF-b-PTFE powder. The weight ratio of the vinylidene fluoride monomer gas and the tetrafluoroethylene monomer gas introduced into the reactor is 1.2:1.

[0038] The above-mentioned initiator is a nitroxide free radical initiator, specifically one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butylbenzene peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

[0039] Step 2: Add the PVDF-b-PTFE powder obtained in step 1 to the N,N-dimethylformamide solution, and stir for 6 hours in a 50° C. water bath to obtain a precursor spinning solution.

[0040] Step 3: Add barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; specifically, the preparation process of the BTO / PVDF-b-PTFE mixed solution is: mix the barium titanate nanoparticles with the precursor spinning solution, and stir for 8 hours in a 70°C water bath; wherein the mass ratio of the barium titanate nanoparticles to the precursor spinning solution is 1:2.

[0041] Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation film, wherein the electrostatic voltage of the electrospinning is 80 kV, the receiving distance is 10 cm, the perfusion rate is 600 mL / h, the spinning temperature is 25° C., and the relative humidity is 50%.

[0042] The porous thermal insulation film prepared by electrospinning in the present invention is a BTO / PVDF-b-PTFE nanofiber thermal insulation film with good durability, which can effectively block infrared and ultraviolet rays for a long time and significantly reduce the temperature indoors and in the car. The high sunlight reflectivity is as high as 80-99.8% and the high and medium infrared emissivity is as high as 70-99.8%. The temperature inside the car covered with the porous BTO / PVDF-b-PTFE thermal insulation film can be reduced by more than 5-55°C compared with the commercial vehicle cover, and can be reduced by more than 10-80°C compared with the model without fabric covering.

[0043] The present invention does not release harmful substances during the manufacturing and use processes, and the raw materials are relatively easy to recycle and process. It is an environmentally friendly material that can have energy-saving effects. At the same time, it can remain stable under extreme climatic conditions and has strong stability.

[0044] It is worth mentioning that the porous thermal insulation film prepared by the porous thermal insulation film preparation method can be used in automobile films. Specifically, the automobile mold includes at least one layer of porous thermal insulation film prepared by the porous thermal insulation film preparation method.

[0045] Those skilled in the art should understand that the embodiments of the present invention shown in the above description are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functions and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. A method for preparing a porous thermal insulation film, characterized in that: include: Step 1, preparing PVDF-b-PTFE powder; Step 2: adding the PVDF-b-PTFE powder obtained in step 1 to an N,N-dimethylformamide solution, or a mixture of N,N-dimethylformamide and acetone to obtain a precursor spinning solution; Step 3: adding barium titanate nanoparticles to the precursor spinning solution obtained in step 2 to obtain a BTO / PVDF-b-PTFE mixed solution; Step 4: The BTO / PVDF-b-PTFE mixed solution obtained in step 3 is spun by an electrospinning process to obtain a porous thermal insulation membrane.

2. The method for preparing a porous thermal insulation film according to claim 1, characterized in that: The preparation process of PVDF-b-PTFE powder in step 1 is: A1. Add deionized water into the reactor and heat the reactor; A2, adding initiator to the reactor and mixing evenly with a stirrer; A3, adding vinylidene fluoride monomer gas into the reactor, and introducing tetrafluoroethylene monomer gas for pressurization; A4, continue the reaction until the solid content in the reactor reaches 15-25%, stop the reaction and remove the latex-like PVDF-b-PTFE; A5. The latex-like PVDF-b-PTFE obtained above is naturally dried, and after drying, it is ground by a ball mill to obtain PVDF-b-PTFE powder.

3. The method for preparing a porous thermal insulation film according to claim 2, characterized in that: The reactor is a 40-liter reactor; the weight of deionized water is 22.5 kilograms; the heating temperature of the reactor in step A1 is 80° C. and maintained; 100 to 200 grams of initiator are added to the reactor; in step A3, vinylidene fluoride monomer gas is added to the reactor so that the pressure in the reactor reaches 0.35 MPa; and then tetrafluoroethylene monomer gas is introduced until the pressure in the reactor reaches 1.52 MPa.

4. The method for preparing a porous thermal insulation film according to claim 2, characterized in that: The initiator is a nitroxide free radical initiator.

5. The method for preparing a porous thermal insulation film according to claim 4, characterized in that: The nitroxide free radical initiator includes: one of ammonium persulfate, benzoyl oxide, benzoyl bromide peroxide, benzoyl peroxide, phenylacetyl peroxide, n-butyl peroxide acrylate, acryloyl peroxide acrylate, toluene peroxide, tert-butyl peroxide, benzene hydroperoxide, tert-butyl peroxide or N-methylpyrrolidone.

6. The method for preparing a porous thermal insulation film according to claim 2, characterized in that: In step A3, the weight ratio of the vinylidene fluoride monomer gas to the tetrafluoroethylene monomer gas introduced into the reactor is 0.8-1.2:

1.

7. The method for preparing a porous thermal insulation film according to claim 1, characterized in that: The preparation process of the precursor spinning solution in step 2 is: adding PVDF-b-PTFE powder to a mixed solvent of N, N-dimethylformamide and acetone, and stirring for 2-6 hours in a water bath at 50-80°C; wherein the volume ratio of N, N-dimethylformamide to acetone is 1:0-10.

8. The method for preparing a porous thermal insulation film according to claim 1, characterized in that: The preparation process of the BTO / PVDF-b-PTFE mixed solution in step three is: mixing barium titanate nanoparticles with the precursor spinning solution, and stirring for 6 to 12 hours in a water bath at 40 to 70°C; wherein the mass ratio of barium titanate nanoparticles to the precursor spinning solution is 1:2 to 10.

9. The method for preparing a porous thermal insulation film according to claim 1, characterized in that: In step 4, the electrostatic voltage of electrospinning is 20-80 kV, the receiving distance is 10-60 cm, the perfusion rate is 20-1500 mL / h, the spinning temperature is 25-40° C., and the relative humidity is 35%-65%.

10. An automotive film using the porous thermal insulation film preparation method of claim 1 to prepare a porous thermal insulation film, characterized in that: It includes at least one layer of porous thermal insulation film.

Citation Information

Patent Citations

  • Method for polymerizing vinylidene fluoride

    CN103748120A

  • Vinylidene fluoride polymer, and preparation method and application thereof

    CN105754027A

  • Gel polymer electrolyte and preparation method and application thereof

    CN113258131A

  • PVDF-BTO composite film and preparation method and application thereof

    CN116874873A

  • Light and thin radiation cooling film and preparation method and application thereof

    CN117306093A