Method for jointly measuring contents of silicon and calcium in silicon-calcium alloy

The silicon and calcium content in the silicon calcium alloy was determined by filter paper and precipitation, which solved the problems of long detection cycles and complex operation in the prior art, achieved fast and accurate results, and avoided the use of harmful substances, improving operational safety.

CN119044396APending Publication Date: 2024-11-29LVLIANG JIANLONG IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411183690.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The methods for detecting the silicon and calcium content in silicon calcium alloys in the prior art need to be measured separately, with a long period and cumbersome operation, and need to be exposed to harmful substances such as sodium peroxide and hydrofluoric acid.

Method used

The combined determination method of filter paper and precipitation was adopted to determine the silicon content by using filter paper and precipitation during the melting process, and the calcium content was determined by EDTA standard titration using filtrate, avoiding the use of highly corrosive reagents and simplifying the operation steps.

Benefits of technology

The simultaneous determination of silicon and calcium content is achieved, with a short detection cycle and accurate results, avoiding the use of strong oxidative and highly corrosive reagents, and improving operational safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012929060000021
    Figure BDA0005012929060000021
  • Figure BDA0005012929060000022
    Figure BDA0005012929060000022
  • Figure BDA0005012929060000031
    Figure BDA0005012929060000031
Patent Text Reader

Abstract

The invention provides a method for simultaneously measuring the contents of silicon and calcium in a silicon-calcium alloy, which comprises the following steps of: melting a sample by using a mixed solvent of anhydrous sodium carbonate and boric acid, adding hydrochloric acid and perchloric acid, evaporating until the mixture is nearly dry, generating insoluble silicic acid from silicon, adding hydrochloric acid and hot water to dissolve other components, and filtering to obtain the content of silicon and calcium in the silicon-calcium alloy. The content of silicon can be calculated after the filter paper and the precipitate are burnt and weighed; adding triethanolamine, potassium hydroxide and a calcium indicator after the filtrate is subjected to volume metering and transferring, titrating with an EDTA standard titration solution, and calculating the mass fraction of calcium according to the consumption of the EDTA standard titration solution. According to the method, the determination of the two elements is realized through one-time melting, the filter paper and the precipitate are used for determining the silicon content, the filtrate is used for determining the calcium content, the detection period is short, the result is accurate, and the use of a strong oxidizing corrosive reagent sodium peroxide and strong corrosive hydrofluoric acid can be avoided in the detection process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical analysis of steel alloys, and in particular to a method for jointly determining the silicon and calcium contents in a silicon-calcium alloy. Background Art

[0002] In the steel industry, calcium silicon alloy is widely used as a deoxidizer and desulfurizer for high-quality steel, low-carbon steel, stainless steel and other steels. Calcium silicon alloy not only has a strong deoxidation ability, and the deoxidation products are easy to float and discharge, but also can improve the performance of steel, improve the plasticity, impact toughness and fluidity of steel. Therefore, the detection of silicon and calcium content in calcium silicon alloy is a necessary means for enterprise product quality certification.

[0003] At present, the determination of silicon content in silicon-calcium alloy mainly adopts the "YB / T 5312-2016 perchloric acid dehydration weight method". After the sample is melted and leached with a mixed flux of sodium peroxide and anhydrous sodium carbonate, hydrochloric acid and perchloric acid are added to smoke, and heated and evaporated to make silicon generate insoluble silicic acid. After burning and weighing, it is treated with hydrofluoric acid to volatilize silicon dioxide, and then burned and weighed. The mass fraction of silicon is calculated based on the difference in mass before and after hydrofluoric acid treatment. The determination of calcium content in silicon-calcium alloy mainly adopts the "YB / T 5313-2016 EDTA titration method". The sample is dissolved with nitric acid and hydrofluoric acid, perchloric acid smoke is used to remove fluoride ions, dissolved with hydrochloric acid, and neutralized and filtered with ammonia to separate impurities such as iron. Then, when the pH is not less than 12, a calcium indicator is added, and the EDTA standard titration solution is used for titration. The mass fraction of calcium is calculated based on the consumption of the EDTA standard titration solution. The method for determining the silicon content and calcium content in the silicon-calcium alloy is to determine them separately, which results in a long detection period and complicated operation. Therefore, the present invention provides a method for jointly determining the silicon and calcium contents in the silicon-calcium alloy. Summary of the invention

[0004] The present invention attempts to provide a method for jointly determining the silicon and calcium contents in a silicon-calcium alloy, which has accurate results, a short detection cycle, and avoids contact with harmful substances.

[0005] The present invention provides a method for jointly determining the silicon and calcium contents in a silicon-calcium alloy, comprising:

[0006] Step 1: Fill a porcelain crucible with high-purity graphite powder, and squeeze the graphite powder in the porcelain crucible to form a graphite inner wall;

[0007] Step 2: Fold 1 / 4 medium-speed filter paper into a cone shape and put it into the mixed flux, weigh the pre-dried sample, mix the sample with the flux, cover it with a layer of flux, wrap the filter paper tightly and put it into a porcelain crucible;

[0008] Step 3: Put the porcelain crucible into a high-temperature furnace, burn for 30 minutes when the temperature reaches 800-900℃, then take it out and cool it. Put the melt into a glass beaker containing hydrochloric acid A and perchloric acid, cover it with a watch glass and evaporate it until it is almost dry. Remove it and rinse the watch glass and beaker with hot hydrochloric acid B, then add hydrochloric acid A and hot water to boil;

[0009] Step 4: After boiling, remove the beaker, filter the material in the beaker with medium-speed quantitative filter paper into another beaker, rinse the original beaker and filter paper with hot hydrochloric acid B three times each, then rinse the original beaker and filter paper with hot water until neutral, transfer the filtrate to a volumetric flask, dilute with water to the scale, and mix well;

[0010] Step 5: Place the filter paper and the precipitate in a porcelain crucible that has been fired to a constant weight and ashed on a low-temperature electric hot plate, then burn in a high-temperature furnace at 800-900°C for 2 hours, take out and cool to room temperature, weigh, and calculate the silicon content in the silicon-calcium alloy. The calculation formula is as shown in Formula 1;

[0011] Step 6: Take a portion of the filtrate in the volumetric flask, add triethanolamine solution and potassium hydroxide solution, add calcium indicator, and titrate with EDTA standard solution until pure blue is the end point. The calcium content in the silicon-calcium alloy can be calculated. The calculation formula is as shown in Formula 2;

[0012] Formula 1:

[0013]

[0014] m1-the mass of the crucible before treatment, g;

[0015] m2-mass of crucible and precipitate after treatment, g;

[0016] m-the amount of sample, g;

[0017] 0.4674 - coefficient for converting silicon dioxide to silicon;

[0018] Formula 2:

[0019]

[0020] c-Concentration of EDTA standard solution, mol / L (the concentration of EDTA standard solution was calibrated with zinc standard solution, and the concentration of EDTA standard solution was measured to be 0.01571 mol / L);

[0021] V1-volume of EDTA standard solution consumed by titration sample, mL;

[0022] k-40.08, molar mass of calcium, g / mol;

[0023] m-the amount of sample, g;

[0024] r-test solution fraction ratio.

[0025] The present invention uses filter paper and precipitation to determine the silicon content and uses filtrate to determine the calcium content. The silicon and calcium contents can be simultaneously determined through only one melting. The detection cycle is short and the detection speed is fast. The use of highly corrosive reagents such as sodium peroxide and hydrofluoric acid is avoided, and the operation is safe. DETAILED DESCRIPTION

[0026] In order to provide a further understanding of the purpose, structure, features, and functions of the present invention, the following detailed description is given in conjunction with the embodiments.

[0027] The invention provides a method for simultaneously determining the content of silicon and calcium in a silicon-calcium alloy. After the sample is melted with a mixed flux of anhydrous sodium carbonate and boric acid, hydrochloric acid and perchloric acid are added to evaporate to near dryness so that silicon generates insoluble silicic acid, and then hydrochloric acid and hot water are added to dissolve the remaining components, and the filter paper and the precipitate are burned and weighed to calculate the content of silicon. After the filtrate is fixed to volume and removed, triethanolamine, potassium hydroxide and calcium indicator are added, and titration is performed with an EDTA standard titration solution. According to the consumption of the EDTA standard titration solution, the mass fraction of calcium is calculated. The method has a short detection cycle and accurate results, and can avoid the use of sodium peroxide, a strongly oxidizing corrosive reagent, and highly corrosive hydrofluoric acid in the detection process.

[0028] The specific steps are as follows:

[0029] (1) Take a 50mL porcelain crucible and fill it with high-purity graphite powder. Then use a 30mL porcelain crucible to squeeze the graphite powder in the 50mL porcelain crucible to form a graphite inner wall, which makes it easier to melt the sample into a spherical shape and remove it.

[0030] (2) Fold 1 / 4 medium-speed filter paper into a cone shape and put in 2g of mixed flux (mixed with anhydrous sodium carbonate and boric acid, by weight, anhydrous sodium carbonate: boric acid = 2:1) to promote the sample into a molten state. Weigh 0.2000g of pre-dried sample (accurate to 0.0001g) and mix it with the flux, then cover it with a layer of flux, wrap it tightly with filter paper and put it in a 50mL porcelain crucible. Perform a blank experiment together with the sample.

[0031] (3) Place the crucible in a high-temperature furnace. When the temperature reaches 800-900°C, burn for 30 minutes, then take it out and cool it (the molten material is now in a ball-like shape). Place the molten material in a 400-mL glass beaker containing 40 mL of hydrochloric acid A (1+1, i.e., the volume ratio of concentrated hydrochloric acid to water is 1:1) and 20 mL of perchloric acid. Cover with a watch glass and evaporate until almost dry. Remove the watch glass and beaker and rinse them with hot hydrochloric acid B (5+95, i.e., the volume ratio of concentrated hydrochloric acid to water is 5:95). Then add 30 mL of hydrochloric acid A (1+1) and 50 mL of hot water and boil them.

[0032] (4) After boiling, remove the beaker and filter the contents through medium-speed quantitative filter paper into a 300-mL beaker. Rinse the beaker and filter paper three times each with hot hydrochloric acid B (5+95), then rinse with hot water until neutral. Transfer the filtrate to a 250-mL volumetric flask, dilute to the mark with water, and mix well.

[0033] (5) Place the filter paper and the precipitate in a porcelain crucible that has been fired to a constant weight and incinerate on a low-temperature electric hot plate. Then, burn them in a high-temperature furnace at 800-900°C for 2 hours. Take them out, cool them to room temperature, and weigh them. The silicon content in the silicon-calcium alloy can be calculated using the formula (1).

[0034] (6) Take 25 mL of the filtrate in the 250 mL volumetric flask, add 5 mL of triethanolamine solution (1+2, i.e., the volume ratio of triethanolamine to water is 1:2) and 20 mL of potassium hydroxide solution (20 g / L), add calcium indicator, and titrate with EDTA standard solution until pure blue is the end point. The calcium content in the silicon-calcium alloy can be calculated. The calculation formula is as shown in Formula 2.

[0035] Formula 1:

[0036]

[0037] m1-the mass of the crucible before treatment, g;

[0038] m2-mass of crucible and precipitate after treatment, g;

[0039] m-the amount of sample, g;

[0040] 0.4674 - The conversion factor of silicon dioxide to silicon.

[0041] Formula 2:

[0042]

[0043] c-Concentration of EDTA standard solution, mol / L (the concentration of EDTA standard solution was calibrated with zinc standard solution, and the concentration of EDTA standard solution was measured to be 0.01571 mol / L);

[0044] V1-volume of EDTA standard solution consumed by titration sample, mL;

[0045] k-40.08, molar mass of calcium, g / mol;

[0046] m-the amount of sample, g;

[0047] r-test solution fraction ratio.

[0048] Experimental data

[0049] First experiment:

[0050] Table 1 Determination of silicon content

[0051]

[0052] Table 2 Determination of calcium content

[0053] Serial number Standard sample name Standard sample number Sample weight Transfer volume / mL <![CDATA[Volume of titrant V1 / mL]]> Measured value Standard value Result bias 1 blank / 0.0000 25 0.00 0.00 / / 2 Silicon calcium alloy QD10-122 0.1999 25 8.90 28.03 28.25 -0.22 3 Silicon calcium alloy QD10-122 0.1999 25 8.90 28.03 28.25 -0.22 4 Silicon calcium alloy QD10-122 0.2001 25 9.00 28.32 28.25 0.07 5 Silicon calcium alloy GBW01431a 0.2002 25 9.70 30.51 30.45 0.06

[0054] Second experiment:

[0055] Table 3 Determination of silicon content

[0056]

[0057]

[0058] Table 4 Determination of calcium content

[0059] Serial number Standard sample name Standard sample number Sample weight Transfer volume / mL <![CDATA[Titration volume V1 / mL]]> Measured value Standard value Result bias 1 blank / 0.0000 25 0.00 0.00 / / 2 Silicon calcium alloy QD10-122 0.2001 25 9.00 28.32 28.25 0.07 3 Silicon calcium alloy YSBC37662-12 0.2001 25 8.00 25.17 25.25 -0.08 4 Silicon calcium alloy YSBC37662-12 0.2003 25 8.10 25.46 25.25 0.21

[0060] The third experiment:

[0061] Table 5 Determination of silicon content

[0062]

[0063] Table 6 Determination of calcium content

[0064] Serial number Standard sample name Standard sample number Sample weight Transfer volume / mL <![CDATA[Titration volume V1 / mL]]> Measured value Standard value Result bias 1 blank / 0.0000 25 0.00 0.00 / / 2 Silicon calcium alloy GBW01431a 0.2001 25 9.70 30.52 30.45 0.07 3 Silicon calcium alloy GBW01431a 0.2000 25 9.70 30.54 30.45 0.09 4 Silicon calcium alloy YSBC37662-12 0.2000 25 8.00 25.19 25.25 -0.06 5 Silicon calcium alloy YSBC37662-12 0.2002 25 8.10 25.48 25.25 0.23

[0065] The allowable difference specified in the standard:

[0066] Table 7 Allowable difference

[0067] Silicon content Allowable difference ≥50.00 0.60 Calcium content Allowable difference 20.00-25.00 0.40 >25.00-36.00 0.50

[0068] From the calculation results of Table 1, Table 2, Table 3, Table 4, Table 5, and Table 6, it can be seen that the values ​​of silicon content and calcium content measured by this method are within the allowable difference range with the standard values, and the measurement results are accurate, so this method is feasible. The results of the present invention are accurate, the determination of silicon content and calcium content can be carried out simultaneously, the detection cycle is short, the detection speed is fast, and the use of highly oxidizing and corrosive sodium peroxide and highly corrosive hydrofluoric acid is avoided, and the operation is safe.

[0069] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the spirit and scope of the present invention are all within the scope of patent protection of the present invention.

Claims

1. A method for jointly determining the silicon and calcium contents in a silicon-calcium alloy, characterized in that: include: Step 1: Fill a porcelain crucible with high-purity graphite powder, and squeeze the graphite powder in the porcelain crucible to form a graphite inner wall; Step 2: Fold 1 / 4 medium-speed filter paper into a cone shape and put it into the mixed flux, weigh the pre-dried sample, mix the sample with the flux, cover it with a layer of flux, wrap the filter paper tightly and put it into a porcelain crucible; Step 3: Put the porcelain crucible into a high-temperature furnace, burn for 30 minutes when the temperature reaches 800-900℃, then take it out and cool it. Put the melt into a glass beaker containing hydrochloric acid A and perchloric acid, cover it with a watch glass and evaporate it until it is almost dry. Remove it and rinse the watch glass and beaker with hot hydrochloric acid B, then add hydrochloric acid A and hot water to boil; Step 4: After boiling, remove the beaker, filter the material in the beaker with medium-speed quantitative filter paper into another beaker, rinse the original beaker and filter paper with hot hydrochloric acid B three times each, then rinse the original beaker and filter paper with hot water until neutral, transfer the filtrate to a volumetric flask, dilute with water to the scale, and mix well; Step 5: Place the filter paper and the precipitate in a porcelain crucible that has been fired to a constant weight and ashed on a low-temperature electric hot plate, then burn in a high-temperature furnace at 800-900°C for 2 hours, take out and cool to room temperature, weigh, and calculate the silicon content in the silicon-calcium alloy. The calculation formula is as shown in Formula 1; Step 6: Take a portion of the filtrate in the volumetric flask, add triethanolamine solution and potassium hydroxide solution, add calcium indicator, and titrate with EDTA standard solution until pure blue is the end point. The calcium content in the silicon-calcium alloy can be calculated. The calculation formula is as shown in Formula 2; Formula 1: m1-the mass of the crucible before treatment, g; m2-mass of crucible and precipitate after treatment, g; m-the amount of sample, g; 0.4674 - coefficient for converting silicon dioxide to silicon; Formula 2: c-Concentration of EDTA standard solution, mol / L (the concentration of EDTA standard solution was calibrated with zinc standard solution, and the concentration of EDTA standard solution was measured to be 0.01571 mol / L); V1-volume of EDTA standard solution consumed by titration sample, mL; k-40.08, molar mass of calcium, g / mol; m-the amount of sample, g; r-test solution fraction ratio.

2. The method for jointly determining the content of silicon and calcium in a silicon-calcium alloy according to claim 1, characterized in that: The mixed flux in step 2 is prepared by mixing anhydrous sodium carbonate and boric acid, with anhydrous sodium carbonate:boric acid=2:1 by weight.

3. The method for jointly determining the content of silicon and calcium in silicon-calcium alloy according to claim 2, characterized in that: Hydrochloric acid A is prepared by using concentrated hydrochloric acid and water in a volume ratio of 1:1, and hydrochloric acid B is prepared by using concentrated hydrochloric acid and water in a volume ratio of 5:

95.

4. The method for jointly determining the content of silicon and calcium in a silicon-calcium alloy according to claim 3, characterized in that: The triethanolamine solution is prepared by mixing triethanolamine and water in a volume ratio of 1:

2.

5. The method for jointly determining the content of silicon and calcium in silicon-calcium alloy according to claim 4, characterized in that: include: Step 1: Take a 50mL porcelain crucible and fill it with high-purity graphite powder, and then use a 30mL porcelain crucible to squeeze the graphite powder in the 50mL porcelain crucible to form a graphite inner wall; Step 2: Fold 1 / 4 medium-speed filter paper into a cone shape and put in 2g of mixed flux, weigh 0.2000g of pre-dried sample (accurate to 0.0001g), mix it with the flux, cover it with a layer of flux, wrap the filter paper tightly and put it in a 50mL porcelain crucible; Step 3: Place the crucible in a high-temperature furnace. When the temperature reaches 800-900°C, burn for 30 minutes, then take it out and cool it. Place the melt in a 400mL glass beaker containing 40mL hydrochloric acid A and 20mL perchloric acid. Cover with a watch glass and evaporate until almost dry. Remove and rinse the watch glass and beaker with hot hydrochloric acid B, then add 30mL hydrochloric acid A and 50mL hot water and boil. Step 4: After boiling, remove the beaker, filter the contents of the beaker with medium-speed quantitative filter paper into a 300 mL beaker, rinse the beaker and filter paper with hot hydrochloric acid B three times each, then rinse with hot water until neutral, transfer the filtrate to a 250 mL volumetric flask, dilute to the mark with water, and mix well; Step 5: Place the filter paper and the precipitate in a porcelain crucible that has been fired to a constant weight and ashed on a low-temperature electric hot plate, then burn in a high-temperature furnace at 800-900°C for 2 hours, take out and cool to room temperature, weigh, and calculate the silicon content in the silicon-calcium alloy. The calculation formula is as shown in Formula 1; Step 6: Pipette 25 mL of the filtrate in the 250 mL volumetric flask, add 5 mL of triethanolamine solution, 20 mL of potassium hydroxide solution (20 g / L), add calcium indicator, and titrate with EDTA standard solution until pure blue is the end point. The calcium content in the silicon-calcium alloy can be calculated. The calculation formula is as shown in Formula 2. Formula 1: m1-the mass of the crucible before treatment, g; m2-mass of crucible and precipitate after treatment, g; m-the amount of sample, g; 0.4674 - coefficient for converting silicon dioxide to silicon; Formula 2: c-Concentration of EDTA standard solution, mol / L (the concentration of EDTA standard solution was calibrated with zinc standard solution, and the concentration of EDTA standard solution was measured to be 0.01571 mol / L); V1-volume of EDTA standard solution consumed by titration sample, mL; k-40.08, molar mass of calcium, g / mol; m-the amount of sample, g; r-test solution fraction ratio.

Citation Information

Patent Citations

  • Method for measuring contents of silicon-calcium elements in silicon-calcium alloy

    CN102213704A

  • Method for measuring silicon in soil and sediment

    CN107505275A

  • Method for determining component content in high-efficiency reducing agent of ladle refining furnace

    CN109406497A

  • Method for detecting calcium and magnesium in sinter

    CN112415129A

  • Method for analyzing aluminum, iron, silicon and phosphorus in aluminum-iron alloy through X-ray fluorescence spectrometry

    CN117169266A