Preparation method of positive electrode pre-lithiation material capable of inhibiting gas production
By covering the oxygen trapping agent on the surface of the positive electrode prelithiated material, the interface problems caused by oxygen production in lithium-ion batteries are solved, the battery energy density and life are improved, and more stable battery performance is achieved.
Patent Information
- Application Number
- CN202411195636.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
The growth of lithium-ion batteries consumes active lithium on the negative electrode surface, resulting in battery energy loss. The positive electrode prelithiated material Li5FeO4 produces oxygen during the chemical formation process, resulting in cell interface problems and low capacity, affecting the battery's long cycle performance.
The lithium source and iron source are subjected to high-speed ball milling and ultrasonic dispersion with the carbon source and oxygen trapping agent in an organic solvent, and the solvent thermal synthesis reaction is carried out, and tetramethylpiperidine or phosphorous acid is coated after drying in a vacuum oven. Triethyl ester forms a stable oxygen trapping layer and reduces oxygen release.
It effectively inhibits the production of oxygen, forms a protective layer, reduces cell interface problems and long cycle risks, and improves the energy density and battery life of lithium-ion batteries.
Smart Images

Figure CN119050363A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and more specifically, to a method for preparing a positive electrode pre-lithiation material capable of inhibiting gas generation. Background Art
[0002] During the formation of lithium-ion batteries, SEI growth on the negative electrode surface consumes active lithium, resulting in battery energy loss. Through positive electrode pre-lithiation technology, a small amount of positive electrode lithium-rich material can be added during the preparation of positive electrode slurry to compensate for the active lithium, thereby increasing the energy density of lithium-ion batteries. The successful application of lithium supplementation technology in lithium-ion batteries can increase the range and life of electric vehicles.
[0003] The widely studied positive electrode pre-lithiation material Li5FeO4 has a high theoretical capacity, and because of its special anti-fluorite structure, it has irreversible delithiation, making it an ideal cathode lithium supplement additive. However, due to the decomposition reaction of Li5FeO4 itself, Li5FeO4→LiFeO2+ 4Li++O2, oxygen will be produced. Therefore, the oxygen produced in the battery cell formation stage will undergo various complex reactions with the electrolyte, and cause interface problems such as black spots and lithium precipitation at the negative electrode interface of the battery cell, thereby causing low capacity of the lithium-supplemented battery cell and affecting the subsequent long-cycle performance of the battery cell.
[0004] Therefore, the present application proposes a method for preparing a positive electrode pre-lithiation material that can suppress gas generation to solve the above problems. Summary of the invention
[0005] Based on this, in order to solve the problem in the background technology that long standing time will lead to particle deposition and agglomeration and uneven coating on the electrode surface, the present invention proposes a method for preparing a positive electrode pre-lithiation material that can inhibit gas production.
[0006] The purpose and effect of the present invention are achieved by the following specific technical means: A method for preparing a positive electrode pre-lithiation material capable of inhibiting gas generation comprises the following steps: S1: After weighing the lithium source and the iron source, add ball milling beads for high-speed ball milling, mix them evenly, put the mixed materials into a sagger, and introduce inert gas into a tube furnace for high-temperature sintering to obtain a sintered material; S2: grinding and crushing the sintered material, adding it to an organic solvent with a carbon source and an oxygen scavenger, and transferring it to a polytetrafluoroethylene reactor for a solvothermal synthesis reaction after ultrasonic dispersion to obtain a solvothermal reaction slurry; S3: Drying the solvent thermal reaction slurry in a vacuum oven, and then grinding the solid to obtain a tetramethylpiperidine-coated Li5FeO4.
[0007] Further preferably, in step S1, the lithium source is one or a combination of more of LiOH.H2O, Li2CO3, LiNO3, Li2O, and Li2O2.
[0008] Further preferably, in step S1, the iron source is one or a combination of ferroferric oxide, ferrous oxide, ferrous sulfate, ferric chloride, and ferrous hydroxide.
[0009] Further preferably, in step S1, the ratio of lithium source to iron source Li:Fe is one of 5.02:1, 5.04:1, 5.06:1, 5.08:1, and 5.10:1.
[0010] Further preferably, in step S1, the high-speed ball milling mixing process conditions are that the ratio of the total mass of the ball milling beads to the mass of the material is one of 1:1, 1:1.5, and 1:2, wherein the ball milling speed is 500-2000rpm, and the ball milling high-speed mixing time is 4-8h.
[0011] Further preferably, in step S1, the polonium is one of corundum polonium, mullite polonium and high-density graphite polonium.
[0012] Further preferably, in step S1, the inert atmosphere is one of argon, nitrogen, helium and neon.
[0013] Further preferably, in the step S1, the sintering process conditions are 600-850° C. and the sintering time is 10-40 hours.
[0014] Further preferably, in step S2, the carbon source is one or more of coconut shell carbon powder, rice husk carbon powder, litchi wood carbon powder, Super-P conductive carbon black, Hi-Black 30 conductive carbon black, CNTs, graphene oxide, petroleum coke, phenolic resin, polyaniline, KB Ketjen black, CMK-3 ordered mesoporous carbon, and glucose.
[0015] Further preferably, in step S2, the oxygen scavenger is one of tetramethylpiperidine, triethyl phosphite, lithium fluoromalonate borate, lithium difluoroborate, lithium bisborate, and lithium bisoxalate.
[0016] Further preferably, in step S2, the ultrasonic dispersion process conditions are ultrasonic frequency 40-60 Hz, ultrasonic temperature 60-80° C., and ultrasonic dispersion time 40-60 min.
[0017] More preferably, in step S2, the organic solvent is one of N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (DMF), dimethylformamide and dimethyl sulfoxide.
[0018] Further preferably, in step S3, the drying process conditions are a drying temperature of 150-200° C. and a vacuum degree of -0.01 to -0.1 KPa.
[0019] Beneficial effects of the present invention: 1. The present invention coats a layer of oxygen scavenger on the surface of the positive electrode pre-lithiation material to consume the decomposed oxygen and form a stable compound, wherein tetramethylpiperidine absorbs the active oxygen generated by its electrochemical decomposition to form a stable tetramethylpiperidine nitrogen oxide. Since triethyl phosphite has a higher binding energy with oxygen molecules, triethyl phosphite can quickly undergo an oxidation reaction with the oxygen released by the lithium supplement material and form a protective layer on the surface of the lithium supplement material, thereby reducing the release of oxygen. Therefore, the problem of the battery interface caused by oxygen production in the lithium supplement battery and the hidden danger of long circulation can be well solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the oxygen capture mechanism diagram of tetramethylpiperidine.
[0021] Figure 2 This is the oxygen capture mechanism diagram of triethyl phosphite.
[0022] Figure 3 This is a disassembly diagram of the lithium battery cell interface. DETAILED DESCRIPTION
[0023] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail in the specific embodiments. The following embodiments are only examples of implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the scope of the present invention are all within the scope of patent protection of the present invention. Example
[0024] This example is carried out through the following experimental steps S1: Li2O2 and ferric oxide were weighed at a Li:Fe ratio of 5.06:1, and then the total mass of the ball mill and the mass of the material were adjusted to a ratio of 1:1. The ball mill speed was 1500rpm, and the ball mill high-speed mixing time was 4h. After mixing evenly, the mixed materials were placed in a sagger and inert gas was introduced into a tubular furnace for high-temperature sintering.
[0025] S2: The sintered material is ground and crushed, and then added to DMF solvent with glucose and tetramethyl piperidine. The ultrasonic dispersion process conditions are ultrasonic frequency 50HZ, ultrasonic temperature 75℃, and ultrasonic dispersion time 60min. After ultrasonic dispersion is uniform, it is transferred to a polytetrafluoroethylene reactor and the reaction process conditions are temperature 240℃ and reaction time 20h for solvent thermal synthesis reaction. S3: Dry the solvent thermal reaction slurry in a vacuum oven at 180° C. with a vacuum degree of −0.08 MPa, and then grind the solid to obtain a tetramethylpiperidine-coated Li 5 FeO 4 material. Example
[0026] The Li2O2 and ferric oxide described in S1 of Example 1 are replaced with LiOH.H2O and ferrosoferric oxide, and the remaining steps are consistent with the above example to obtain a tetramethylpiperidine-coated Li5FeO4 material. Example
[0027] The glucose in S2 of Example 1 was replaced with graphene oxide, and the remaining steps were consistent with the above example to obtain a tetramethylpiperidine-coated Li5FeO4 Example
[0028] S1: LiOH.H2O and ferroferric oxide were weighed at a Li:Fe ratio of 5.08:1, and then the total mass of the ball mill beads and the mass of the material were adjusted to 1:2. The ball mill speed was 1500rpm, and the ball mill high-speed mixing time was 4h. After mixing evenly, the mixed material was placed in a sagger, and inert gas was introduced into a tubular furnace for high-temperature sintering to obtain a sintered material.
[0029] S2: Grind the above sintered material and add it into NMP solvent with graphene oxide and triethyl phosphite. The ultrasonic dispersion process conditions are ultrasonic frequency 50HZ, ultrasonic temperature 75℃, ultrasonic dispersion time 60min. After ultrasonic dispersion is uniform, transfer it to a polytetrafluoroethylene reactor and carry out solvent thermal synthesis reaction at reaction process conditions of temperature 240℃ and reaction time 20h to obtain solvent thermal reaction slurry.
[0030] S3: Dry the solvent thermal reaction slurry in a vacuum oven at 180° C. with a vacuum degree of −0.08 MPa, and then grind the solid to obtain a triethyl phosphite-coated Li 5 FeO 4 material. Example
[0031] The triethyl phosphite described in S2 of Example 4 is replaced with LiFMDFB, and the remaining steps are consistent with those of Example 4 to obtain a LiFMDFB-coated Li5FeO4 material. Example
[0032] The triethyl phosphite described in S2 of Example 4 is replaced with LiBOB, and the remaining steps are consistent with those of Example 4, so as to obtain a LiBOB-coated Li5FeO4 material.
[0033] Comparative Example 1: LiOH.H2O and ferroferric oxide were weighed at a Li:Fe ratio of 5.08:1, and then the total mass of the ball mill beads and the mass of the material were adjusted to a ratio of 1:2. The ball mill speed was 1500rpm, and the ball mill high-speed mixing time was 4h. After mixing evenly, the mixed material was placed in a sagger, and an inert gas was introduced into a tubular furnace for high-temperature sintering to obtain the sintered material to obtain Li5FeO4 material.
[0034] The finished materials prepared in all the embodiments and comparative examples are made into soft-pack batteries, which need to go through the steps of slurrying, coating, drying, rolling, winding, heat sealing, formation, and cabinet testing: ① Prepare slurry, weigh the positive electrode material and lithium supplement additive, conductive agent, and binder respectively, and mix them, wherein the mass ratio of positive electrode material: lithium supplement additive: conductive agent: binder is 95:2.5:1.5:1, the binder used is PVDF, and the conductive agent is conductive carbon; ② Coating, use a transfer coater to coat on aluminum foil; ③ Drying, dry the coated electrode sheet in a vacuum drying oven at 90°C; ④ Rolling, press the dried electrode sheet through a roller machine; ⑤ Wind the positive electrode sheet, negative electrode sheet, diaphragm, and other battery parts into a small soft-pack battery cell. The formation test was carried out under the conditions of charging voltage range of 2.5-4.2V and charging rate of 0.1C to test the catalytic gram capacity of the lithium supplement agent and the gas production volume of the battery cell. At the same time, the battery cell after formation was disassembled to analyze the interface of the electrode. The interface conditions are as follows Figure 3 The test results are summarized in the following table.
[0035] Group Lithium Supplement Catalytic Gram Capacity (mAh / g) Gas Production Volume (mL) Group Lithium supplement catalytic gram capacity (mAh / g) Gas production volume (mL) Comparative Example 1 463 31.8 Example 1 658 20.3 Example 2 684 20.9 Example 3 723 21.7 Example 4 715 18.6 Example 5 693 23.8 Example 6 689 22.7 Table 1 Through the analysis of the gram capacity data of the lithium replenisher catalysis in the above table, it can be obtained that a better carbon source is conducive to constructing a carbon layer conductive network with excellent lithium ion conductivity on the surface of the pre-lithiation material, which can reduce the polarization problem of the electrochemical catalysis of the material and enhance the gram capacity of the lithium replenisher at the battery end. On the other hand, by introducing the oxygen capture layer material on the surface of the lithium replenisher material through the oxidation reaction with oxygen to form a stable and beneficial solid SEI film component, the gas production volume at the application end of the battery cell can be significantly reduced, and the interface energy of the lithium replenisher battery cell can be well improved, thereby solving the hidden dangers of the subsequent long cycle performance of the lithium replenisher battery cell.
Claims
1. A method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation, characterized in that: The following steps are involved: S1: After weighing the lithium source and the iron source, add ball milling beads for high-speed ball milling, mix them evenly, put the mixed materials into a sagger, and introduce inert gas into a tube furnace for high-temperature sintering to obtain a sintered material; S2: grinding and crushing the sintered material, adding it to an organic solvent with a carbon source and an oxygen scavenger, and transferring it to a polytetrafluoroethylene reactor for a solvothermal synthesis reaction after ultrasonic dispersion to obtain a solvothermal reaction slurry; S3: Drying the solvent thermal reaction slurry in a vacuum oven, and then grinding the solid to obtain a tetramethylpiperidine-coated Li5FeO4.
2. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In step S1, the lithium source is one or a combination of LiOH.H2O, Li2CO3, LiNO3, Li2O, and Li2O2.
3. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S1, the iron source is one or a combination of ferroferric oxide, ferrous oxide, ferrous sulfate, ferric chloride, and ferrous hydroxide.
4. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S1, the ratio of lithium source to iron source Li:Fe is one of 5.02:1, 5.04:1, 5.06:1, 5.08:1, and 5.10:
1.
5. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In step S1, the high-speed ball milling mixing process conditions are that the ratio of the total mass of the ball milling beads to the mass of the material is one of 1:1, 1:1.5, and 1:2, wherein the ball milling speed is 500-2000rpm, and the ball milling high-speed mixing time is 4-8h.
6. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S1, the polonium is one of corundum polonium, mullite polonium, and high-density graphite polonium.
7. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S1, the inert atmosphere is one of argon, nitrogen, helium, and neon.
8. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S1, the sintering process conditions are 600-850° C. and the sintering time is 10-40 hours.
9. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In step S2, the carbon source is one or more of coconut shell carbon powder, rice husk carbon powder, litchi wood carbon powder, Super-P conductive carbon black, Hi-Black 30 conductive carbon black, CNTs, graphene oxide, petroleum coke, phenolic resin, polyaniline, KB Ketjen black, CMK-3 ordered mesoporous carbon, and glucose.
10. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In step S2, the oxygen scavenger is one of tetramethyl piperidine, triethyl phosphite, lithium fluoromalonate borate, lithium difluoroborate, lithium bisborate, and lithium bisoxalate.
11. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S2, the ultrasonic dispersion process conditions are as follows: ultrasonic frequency 40-60 Hz, ultrasonic temperature 60-80° C., and ultrasonic dispersion time 40-60 min.
12. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In the step S2, the organic solvent is one of N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (DMF), dimethylformamide, and dimethyl sulfoxide.
13. The method for preparing a positive electrode pre-lithiation material capable of suppressing gas generation according to claim 1, characterized in that: In step S3, the drying process conditions are a drying temperature of 150-200° C. and a vacuum degree of -0.01 to -0.1 Kpa.
Citation Information
Cited By
Lithium supplement agent and preparation method thereof, positive plate, lithium ion battery, battery pack and electric equipment
CN120497343A