Protective film layer, lithium electrode, preparation method of lithium electrode and lithium battery

By using a protective film layer of oxygen-containing or nitrogen-containing polar polymer and inorganic filler particles on the lithium metal electrode, the poor environmental adaptability and safety problems of the lithium metal electrode are solved, extending the electrode life and reducing production costs.

CN119050365APending Publication Date: 2024-11-29ADVANCED MATERIALS TECH (BEIJING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411336208.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Lithium metal electrodes have a reactive reaction with water, carbon dioxide and oxygen in the air, resulting in safety problems and poor environmental adaptability, which limits their industrial application and increases production costs.

Method used

Polar polymers containing oxygen-containing polar groups and/or nitrogen-containing polar groups are coordinated and combined with inorganic filler particles to form channels that are conducive to lithium ion transfer and cooperate with non-polar organic matter to form isolated water and gas The dense film layer is used as a protective film layer for lithium metal electrodes to improve lithium ion conductivity and oxidation resistance.

Benefits of technology

It effectively alleviates the erosion of lithium metal electrodes in the air, extends life, reduces production costs, and improves the environmental adaptability and electrical performance of lithium metal electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005058308850000081
    Figure BDA0005058308850000081
  • Figure BDA0005058308850000091
    Figure BDA0005058308850000091
Patent Text Reader

Abstract

The invention provides a protective film layer, a lithium electrode, a preparation method of the lithium electrode and a lithium battery. The protective film layer comprises a non-polar organic matter, a polar polymer and inorganic filler particles, and the weight ratio of the non-polar organic matter to the polar polymer to the inorganic filler particles is (10-25): (1-10): (0.5-5); the non-polar organic matter is selected from at least one of a non-polar polymer and paraffin with 20-40 carbon atoms; the polar polymer has an oxygen-containing polar group and / or a nitrogen-containing polar group. Based on the protective film layer, the problem of poor environmental adaptability of a lithium metal electrode in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a protective film layer, a lithium electrode and a preparation method thereof, and a lithium battery. Background Art

[0002] With the rapid consumption of non-renewable fossil fuels and the continuous deterioration of the environment, replacing fossil fuels with green new energy has become a major research direction. Lithium batteries, with their high energy density, can not only provide ideal energy for portable electronic products such as mobile phones and computers, but also meet the high safety, high energy density and high rate requirements of future new energy electric vehicles. They are playing an increasingly important role in people's lives with their irreplaceable advantages.

[0003] Lithium metal is used as negative electrode material due to its high theoretical capacity and low potential. However, there are still many problems with using lithium metal directly as negative electrode material: lithium metal itself is very active and will react with water, carbon dioxide, oxygen, and nitrogen in the air at room temperature and be consumed. In particular, lithium metal reacts very quickly with water, releasing a large amount of heat and hydrogen, causing huge safety issues. Therefore, the production and assembly of lithium metal needs to be carried out in a dry room with a relative humidity of less than 1%, and the subsequent battery packaging also needs to be carried out in a more stringent inert environment, which limits the industrial application of lithium metal electrodes. In addition, strict storage and assembly conditions will also greatly increase the uncertainty cost of lithium metal negative electrodes. Summary of the invention

[0004] The main purpose of the present invention is to provide a protective film layer, a lithium electrode and a preparation method thereof, and a lithium battery to solve the problem of poor environmental adaptability of lithium metal electrodes in the prior art.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a protective film layer is provided, comprising a non-polar organic matter, a polar polymer, and inorganic filler particles, wherein the weight ratio of the non-polar organic matter, the polar polymer, and the inorganic filler particles is (10-25): (1-10), (0.5-5); the non-polar organic matter is selected from at least one of a non-polar polymer and a chain alkane having twenty to forty carbon atoms; the polar polymer has an oxygen-containing polar group and / or a nitrogen-containing polar group.

[0006] Furthermore, the surface tension of the non-polar organic matter is ≤32 dyn / cm.

[0007] Preferably, the non-polar organic matter is selected from at least one of polyethylene, polypropylene and chlorinated polypropylene.

[0008] Preferably, the polar polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polycarbonate, polyester and polysiloxane.

[0009] Preferably, the material of the inorganic filler particles is at least one selected from alumina, silica, and titanium dioxide.

[0010] Preferably, the weight average molecular weight of the non-polar polymer is 1000-5000, and the weight average molecular weight of the polar polymer is 5000-15000.

[0011] Furthermore, the non-polar organic substance is chlorinated polypropylene, and the polar polymer is polysiloxane; or, the non-polar organic substance is polyethylene, and the polar polymer is polyethylene oxide.

[0012] Preferably, the weight ratio of the non-polar organic matter, the polar polymer and the inorganic filler particles is (15-20):(4-6):(2-5).

[0013] Furthermore, the particle size of the inorganic filler particles is 10≤D90≤100 nm.

[0014] Preferably, the thickness of the protective film layer is 100 nm to 1000 nm.

[0015] Preferably, the thickness of the protective film layer is 400 nm to 600 nm.

[0016] According to another aspect of the present invention, a lithium electrode is provided, comprising a lithium metal layer and a protective film layer coated on at least one side of the lithium metal layer, wherein the protective film layer is the protective film layer as described above.

[0017] According to another aspect of the present invention, there is provided a method for preparing the lithium electrode as above, comprising the following steps:

[0018] Step S1, heating the first organic solvent to 40° C. to 80° C., then adding non-polar organic matter and polar polymer according to a ratio, and dissolving to obtain a mixed solution;

[0019] Step S2, dispersing inorganic filler particles in the mixed solution according to a ratio to obtain a coating slurry;

[0020] Step S3, coating the coating slurry on at least one side of the lithium metal layer, and obtaining a lithium electrode after drying;

[0021] The weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles and the first organic solvent is (10-25): (1-10): (0.5-5): (30-89).

[0022] Furthermore, the first organic solvent is selected from at least one of toluene, xylene, tetrahydrofuran, carbon tetrachloride, and n-heptane.

[0023] Preferably, in step S1, after adding the non-polar organic matter and the polar polymer, stirring is performed for 1 h to 3 h to obtain a mixed solution.

[0024] Furthermore, in step S2, inorganic filler particles are added to the mixed solution, stirred for 2 hours to 5 hours, and then a second organic solvent is added and stirred for 20 minutes to 40 minutes to obtain a coating slurry.

[0025] Preferably, the weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles, the first organic solvent and the second organic solvent is (10-25): (1-10): (0.5-5): (30-45): (30-45).

[0026] Preferably, the second organic solvent is selected from at least one of toluene, xylene, tetrahydrofuran, carbon tetrachloride and n-heptane.

[0027] Preferably, the coating slurry particle size is less than 500 nm.

[0028] Furthermore, the coating method is selected from one of dip coating and roller coating.

[0029] Preferably, the coating method is dipping.

[0030] More preferably, the coating speed of the dip coating is 2 mm / s to 20 mm / s, and further preferably, the coating speed is 5 mm / s to 10 mm / s.

[0031] According to another aspect of the present invention, a lithium battery is provided, the lithium battery comprising the above lithium electrode or a lithium electrode prepared by the above method for preparing a lithium electrode.

[0032] By applying the technical solution of the present invention, polar polymers containing oxygen polar groups and / or nitrogen polar groups are coordinated and combined with inorganic filler particles to form channels that are conducive to lithium ion transmission, and the performance of non-polar organic matter (non-polar polymers, C20-C40 chain alkanes) is easily formed to isolate water and gas. A protective film layer that has both the ability to isolate water and gas and the ability to conduct ions is obtained through the ratio of the three. When the protective film layer is used as a protective film layer for a lithium metal electrode, the lithium metal can be relieved from corrosion by water, carbon dioxide, oxygen, etc. in the air, thereby increasing the life of the lithium metal electrode. At the same time, the protective film layer also has a relatively high lithium ion conductivity, ensuring that the electrical properties of the lithium metal electrode will not be affected after the protective layer is added. In addition, the protective film layer enhances the anti-oxidation properties of lithium metal, which can effectively reduce the corrosion of the lithium metal electrode in the air, so that the lithium metal electrode can better adapt to the storage and assembly environment of existing lithium-ion batteries, which is beneficial to the industrial application of lithium metal electrodes and reduces production costs. DETAILED DESCRIPTION

[0033] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0034] As described in the background art, in the prior art, lithium metal electrodes have the problem of poor environmental adaptability. In order to solve the above problem, according to one aspect of the present invention, a protective film layer is provided, comprising a first polymer, a second polymer, and inorganic filler particles, wherein the weight ratio of the first polymer, the second polymer, and the inorganic filler particles is (10-25): (1-10), (0.5-5); the first polymer is a non-polar polymer; the second polymer is a polar polymer containing oxygen polar groups and / or nitrogen polar groups.

[0035] In order to improve the environmental adaptability of lithium metal electrodes, the present invention provides a protective film layer, which forms a channel that is conducive to the transfer of lithium ions by combining polar polymers containing oxygen polar groups and / or nitrogen polar groups with inorganic filler particles, and combines the performance of non-polar organic matter (non-polar polymers, C20-C40 chain alkanes) to easily form a dense film layer that isolates water and gas. Through the ratio of the three, a protective film layer with the ability to isolate water and gas and ion conductivity is obtained; when the protective film layer is used as a protective film layer for lithium metal electrodes, it can relieve the corrosion of lithium metal by water, carbon dioxide, oxygen, etc. in the air, thereby prolonging the life of the lithium metal electrode; at the same time, the protective film layer also has a high lithium ion conductivity, ensuring that the electrical properties of the lithium metal electrode will not be affected after the protective layer is added; in addition, the protective film layer enhances the anti-oxidation properties of lithium metal, which can effectively reduce the corrosion of lithium metal electrodes in the air, so that the lithium metal electrodes can better adapt to the storage and assembly environment of existing lithium ion batteries, which is beneficial to the industrial application of lithium metal electrodes and reduces production costs.

[0036] In one embodiment, the surface tension of the non-polar organic matter is ≤32dyn / cm, so that the non-polar organic matter has a lower surface energy so that a dense film layer can be formed after drying; preferably, the non-polar organic matter is selected from at least one of polyethylene, polypropylene, and chlorinated polypropylene. The above non-polar polymer is easy to form a film, and by combining with polar polymers and inorganic filler particles, the protective performance and ion conductivity of the protective film layer can be better balanced; preferably, the polar polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polycarbonate, polyester, and polysiloxane. The above polar polymer can form a channel that is more conducive to lithium ion transfer with the inorganic filler particles, improve the directional conduction rate of lithium ions in the electric field, and has good affinity and miscibility with the non-polar polymer. While improving the lithium ion conductivity of the protective film layer, the density and uniformity of the film are guaranteed so that Better isolate water and gas; adding inorganic filler particles can, on the one hand, inhibit polymer crystallization, reduce polymer Tg, and enhance polymer segment movement to improve ion conductivity; on the other hand, inorganic filler particles can form a void structure with non-polar polymers and polar polymers, providing a free channel for lithium ion transfer, thereby further improving product ion conductivity. Preferably, the material of the inorganic filler particles is selected from at least one of aluminum oxide, silicon dioxide, and titanium dioxide to obtain higher lithium ion conductivity; preferably, the weight average molecular weight of the non-polar polymer is 1000-5000, and the weight average molecular weight of the polar polymer is 5000-15000. The polar polymers and non-polar polymers of the above molecular weights have better solubility, and the two have better affinity and miscibility, so as to improve the density and uniformity of film formation and better isolate water and gas.

[0037] In one embodiment, in order to obtain higher ionic conductivity and water vapor isolation performance, the weight ratio of non-polar organic matter, polar polymer and inorganic filler particles is (15-20): (4-6): (2-5); preferably, the non-polar organic matter is chlorinated polypropylene, and the polar polymer is polysiloxane. The combination of polysiloxane and inorganic filler and chlorinated polypropylene has higher lithium ion conductivity, and polysiloxane and chlorinated polypropylene have better affinity and miscibility, and have better film-forming performance; or, the non-polar organic matter is polyethylene, and the polar polymer is polyethylene oxide. The combination of the two and the inorganic filler has higher conductivity, and polyethylene and polyethylene oxide have better affinity and miscibility.

[0038] In one embodiment, the particle size of the inorganic filler particles preferably satisfies: 10≤D90≤100nm. At this particle size, it has good film-forming properties in combination with the polymer to obtain a uniform and dense protective film layer, and at the same time has good ion conductivity so as to obtain higher ion conductivity and higher water vapor isolation performance; the thickness of the protective film layer is preferably 100nm~1000nm; the thickness of the protective film layer is preferably 400nm~600nm, which has better water vapor isolation performance and ion conductivity, while avoiding excessive size of the membrane product to save costs.

[0039] According to another aspect of the present invention, a lithium electrode is provided, comprising a lithium metal layer and a protective film layer coated on at least one side of the lithium metal layer, wherein the protective film layer is the protective film layer as described above.

[0040] According to another aspect of the present invention, a method for preparing a lithium electrode is provided, comprising the following steps: step S1, heating a first organic solvent to 40°C to 80°C, then adding a non-polar organic matter and a polar polymer according to a ratio, dissolving to obtain a mixed solution; step S2, dispersing inorganic filler particles in the mixed solution according to a ratio to obtain a coating slurry; step S3, coating the coating slurry on at least one side of a lithium metal layer, and obtaining a lithium electrode after drying; wherein the weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles and the first organic solvent is (10-25): (1-10): (0.5-5): (30-89). The non-polar organic matter and the second polymer are dissolved under heating conditions to form a uniform solution system, and the inorganic filler particles added subsequently are dispersed to form a stable dispersion system, which is then coated on the lithium metal layer to form a protective film layer having ion conductivity and water vapor isolation performance.

[0041] In one embodiment, the first organic solvent is selected from at least one of toluene, xylene, tetrahydrofuran, carbon tetrachloride, and n-heptane. The above solvents have good film-forming properties and have good solubility properties for polar polymers and non-polar organic matter under heating conditions; preferably, in step S1, after adding the non-polar organic matter and the polar polymer, stir for 1h to 3h to obtain a mixed solution.

[0042] In one embodiment, in step S2, inorganic filler particles are added to the mixed solution, stirred for 2h to 5h, and then the second organic solvent is added and stirred for 20min to 40min to obtain a coating slurry. The solvent is added during the dispersion process to reduce the viscosity of the coating slurry, which is beneficial to subsequent coating. Preferably, the weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles, the first organic solvent and the second organic solvent is (10-25): (1-10): (0.5-5): (30-45): (30-45), and the organic solvent is added in batches. The organic solvent is first used to dissolve the non-polar organic matter and the polar polymer to form a solution system with a certain viscosity, so that the inorganic filler is fully dispersed and forms a stable dispersion system, and then the organic solvent is added to dilute and reduce the viscosity, and the raw materials and the organic solvent are controlled within the above range to facilitate subsequent coating processing and improve the film quality. Preferably, the particle size of the coating slurry is less than 500nm, the film layer has good uniformity and high film quality.

[0043] Furthermore, the coating method is selected from one of dip coating and roller coating; preferably, the coating method is dip coating; more preferably, the coating speed of dip coating is 2 mm / s to 20 mm / s, and further preferably, the coating speed is 5 mm / s to 10 mm / s.

[0044] According to another aspect of the present invention, a lithium battery is provided, comprising a lithium electrode as described above or a lithium electrode prepared by the method for preparing a lithium electrode as described above, wherein the prepared lithium electrode has the ability to isolate water and gas and to conduct ions, has good environmental adaptability, and can stably receive and output lithium ions in the lithium battery.

[0045] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0046] It should be noted that the polysiloxane (DOW Corning 3-2576, USA), polyethylene oxide (Dow EPIKOTE Resin 828, USA), polycarbonate (China Bluestar, AMT291BCR-1000), polyester (Allnex, USA) used in the examples and comparative examples are 26-3705) and chlorinated polypropylene (CP-30) were commercially available.

[0047] Example 1

[0048] A lithium electrode comprises a lithium metal electrode body and a protective film layer coated on both sides of the lithium metal electrode body, wherein the protective film layer comprises chlorinated polypropylene, polysiloxane and aluminum oxide particles, wherein the weight ratio of chlorinated polypropylene, polysiloxane and aluminum oxide particles is 20:5:3, the weight average molecular weight of chlorinated polypropylene is 3000, the weight average molecular weight of polysiloxane is 10000, and the particle size D90 of aluminum oxide particles is 50 nm.

[0049] Specifically, the preparation method of the lithium electrode comprises the following steps:

[0050] Step 1, heating toluene to 60° C., then adding chlorinated polypropylene and polysiloxane according to the ratio, stirring for 2 hours, to obtain a polymer mixed solution;

[0051] Step 2: adding alumina particles to the polymer mixed solution according to the ratio, stirring for 3 hours to obtain a dispersion system of inorganic filler particles, and then adding xylene and stirring for 30 minutes to obtain a coating slurry;

[0052] Step 3, coating the coating slurry on the lithium metal electrode body by dip coating, and drying at 70° C. to form a 500 nm protective film layer to obtain a lithium electrode;

[0053] Among them, the weight ratio of chlorinated polypropylene, toluene and xylene is 20:40:32.

[0054] Example 2

[0055] The difference between it and Example 1 is that the raw material composition of the protective film layer is different, as shown in Table 1.

[0056] Example 3

[0057] A lithium electrode comprises a lithium metal electrode body and a protective film layer coated on both sides of the lithium metal electrode body, wherein the protective film layer comprises polyethylene, polyethylene oxide and silicon dioxide particles, wherein the weight ratio of polyethylene, polyethylene oxide and silicon dioxide particles is 10:1:0.5, the weight average molecular weight of polyethylene is 1000, the weight average molecular weight of polyethylene oxide is 5000, and the particle size D90 of silicon dioxide particles is 10 nm.

[0058] Specifically, the preparation method of the lithium electrode comprises the following steps:

[0059] Step 1, heating toluene to 80° C., then adding polyethylene and polyethylene oxide according to the ratio, stirring for 1 hour, to obtain a polymer mixed solution;

[0060] Step 2: Add silica particles to the polymer mixed solution according to the ratio, stir for 2 hours to obtain a dispersion system of inorganic filler particles, then add toluene and stir for 20 minutes to obtain a coating slurry;

[0061] Step 3, coating the coating slurry on the lithium metal electrode body by dip coating, and drying at 70° C. to form a protective film layer of 100 nm to obtain a lithium electrode;

[0062] Among them, the weight ratio of polyethylene to toluene is 10:70, and the weight ratio of toluene added in step one to toluene added in step two is 30:45.

[0063] Example 4

[0064] A lithium electrode comprises a lithium metal electrode body and a protective film layer coated on both sides of the lithium metal electrode body, wherein the protective film layer comprises polypropylene, polyacrylonitrile and titanium dioxide particles, wherein the weight ratio of the polypropylene, polyacrylonitrile and titanium dioxide particles is 25:10:5, the weight average molecular weight of the polypropylene is 5000, the weight average molecular weight of the polyacrylonitrile is 15000, and the particle size D90 of the titanium dioxide particles is 100 nm.

[0065] Specifically, the preparation method of the lithium electrode comprises the following steps:

[0066] Step 1, heating tetrahydrofuran to 40° C., then adding polypropylene and polyacrylonitrile according to the ratio, stirring for 3 hours, to obtain a polymer mixed solution;

[0067] Step 2: adding titanium dioxide particles to the polymer mixed solution according to the ratio, stirring for 5 hours to obtain a dispersion system of inorganic filler particles, and then adding tetrahydrofuran and stirring for 40 minutes to obtain a coating slurry;

[0068] Step 3, coating the coating slurry on the lithium metal electrode body by dip coating, and drying at 70° C. to form a protective film layer of 1000 nm to obtain a lithium electrode;

[0069] The weight ratio of polypropylene to tetrahydrofuran is 25:70, and the weight ratio of tetrahydrofuran added in step 1 to tetrahydrofuran added in step 2 is 45:30.

[0070] Example 5

[0071] A lithium electrode comprises a lithium metal electrode body and a protective film layer coated on both sides of the lithium metal electrode body, wherein the protective film layer comprises polyethylene, polyacrylonitrile and titanium dioxide particles, wherein the weight ratio of the polyethylene, polyacrylonitrile and titanium dioxide particles is 10:10:4, the weight average molecular weight of the polyethylene is 3000, the weight average molecular weight of the polyacrylonitrile is 10000, and the particle size D90 of the titanium dioxide particles is 50 nm.

[0072] Specifically, the preparation method of the lithium electrode comprises the following steps:

[0073] Step 1, heating xylene to 60° C., then adding polyethylene and polyacrylonitrile according to the ratio, stirring for 2 hours, and obtaining a polymer mixed solution;

[0074] Step 2: adding titanium dioxide particles to the polymer mixed solution according to the ratio, stirring for 3 hours to obtain a dispersion system of titanium dioxide particles and obtain a coating slurry;

[0075] Step 3, coating the coating slurry on the lithium metal electrode body by dip coating, and drying at 70° C. to form a protective film layer of 100 nm to obtain a lithium electrode;

[0076] Among them, the weight ratio of polyethylene to xylene is 20:85.

[0077] Examples 6 to 9

[0078] The difference between it and Example 5 is that the raw material composition of the protective film layer in the lithium electrode is different, the solvent used in the preparation of the lithium electrode and the thickness of the prepared protective film layer are different, see Table 1 for details.

[0079] Example 10

[0080] The difference between this embodiment and Example 1 is that the chlorinated polypropylene is replaced by C20 straight-chain alkane.

[0081] Embodiment 11

[0082] The difference between this embodiment and Example 1 is that the chlorinated polypropylene is replaced by C30 straight-chain alkane.

[0083] Example 12

[0084] The difference between this embodiment and Example 1 is that the chlorinated polypropylene is replaced by C40 straight-chain alkane.

[0085] Embodiment 13

[0086] The difference between this embodiment and Example 1 is that chlorinated polypropylene is replaced by C30 branched alkane (CH 3 ) 2 CH(CH 2 ) 24 CH(CH 3 ) 2 .

[0087] Comparative Example 1

[0088] The difference between this embodiment and Example 1 is that no chlorinated polypropylene is added to the protective film layer.

[0089] Comparative Example 2

[0090] The difference between this embodiment and Example 1 is that no polysiloxane is added to the protective film layer.

[0091] Comparative Example 3

[0092] The difference between this embodiment and Example 1 is that no aluminum oxide particles are added to the protective film layer.

[0093] Comparative Example 4

[0094] The difference between this embodiment and Example 2 is that polyethylene is not added to the protective film layer.

[0095] Comparative Example 5

[0096] The difference between this embodiment and Example 2 is that polyethylene oxide is not added into the protective film layer.

[0097] Comparative Example 6

[0098] The only difference between it and Example 5 is that no titanium dioxide particles are added to the protective film layer.

[0099] Comparative Example 7

[0100] The only difference between it and Example 8 is that no silicon dioxide particles are added to the protective film layer.

[0101] Comparative Example 8

[0102] The only difference from Example 9 is that no aluminum oxide particles are added to the protective film layer.

[0103] Lithium electrode performance test:

[0104] Environmental adaptability test of lithium electrode: The lithium electrodes prepared in the examples and comparative examples were exposed to an atmosphere with a dew point of 30°C and a temperature of 25°C. The black spots on the surface of the lithium metal were observed every 30 minutes, and the time when the black spots first appeared on the surface was recorded. The specific test results are shown in Table 1.

[0105] Ion conductivity test: The ion conductivity of the lithium electrodes prepared in the examples and comparative examples was tested with reference to the ion conductivity test method in GB / T 36363. The specific test results are shown in Table 1.

[0106] Water contact angle test: Using the shape image analysis method, a water drop is dropped on the surface of the solid sample. The shape image of the drop is obtained through the microscope lens and camera, and the contact angle is then calculated through the instrument system. The specific test results are shown in Table 1.

[0107] Table 1

[0108]

[0109]

[0110] It can be seen from Table 1 that the protective film layer prepared in Examples 1-13 of the present invention has high lithium ion conductivity and good hydrophobic and water-isolating properties, and the protective film layer enhances the antioxidant properties of lithium metal and can effectively reduce the corrosion of lithium metal electrodes in the air.

[0111] Compared with Example 1, no chlorinated polypropylene was added in Comparative Example 1. Although the protective film layer has high ionic conductivity, the environmental adaptability of the lithium electrode and the easy corrosion of the metal electrode in the air. Comparative Document 2 did not add polyethylene oxide, and its ionic conductivity was extremely poor. No aluminum oxide particles were added in Comparative Example 3, and its ionic conductivity was significantly reduced.

[0112] Compared with Example 2, Comparative Example 4 does not add polyethylene, which has extremely high electrical conductivity but is extremely susceptible to corrosion in the air. Comparative Example 5 does not add polyethylene oxide, and its ionic conductivity is extremely poor.

[0113] Compared with Example 5, Comparative Example 6 did not add polyethylene oxide, and its ion conductivity was extremely poor.

[0114] Compared with Example 8, no silicon dioxide particles were added in Comparative Example 7, and its ion conductivity decreased.

[0115] Compared with Example 9, in Comparative Example 8, no alumina particles were added, and its ionic conductivity was significantly reduced.

[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A protective film layer, It is characterized in that It includes non-polar organic matter, polar polymer, and inorganic filler particles, wherein the weight ratio of the non-polar organic matter, the polar polymer, and the inorganic filler particles is (10-25): (1-10), (0.5-5); the non-polar organic matter is selected from at least one of a non-polar polymer and a chain alkane having twenty to forty carbon atoms; the polar polymer has an oxygen-containing polar group and / or a nitrogen-containing polar group.

2. The protective film layer according to claim 1, It is characterized in that The surface tension of the non-polar organic matter is ≤32dyn / cm; Preferably, the non-polar organic matter is selected from at least one of polyethylene, polypropylene, and chlorinated polypropylene; Preferably, the polar polymer is selected from at least one of polyethylene oxide, polyacrylonitrile, polycarbonate, polyester, and polysiloxane; Preferably, the material of the inorganic filler particles is selected from at least one of alumina, silica and titanium dioxide; Preferably, the weight average molecular weight of the non-polar polymer is 1000-5000, and the weight average molecular weight of the polar polymer is 5000-15000.

3. The protective film layer according to claim 2, It is characterized in that The non-polar organic substance is chlorinated polypropylene, and the polar polymer is polysiloxane; or, the non-polar organic substance is polyethylene, and the polar polymer is polyethylene oxide; Preferably, the weight ratio of the non-polar organic matter, the polar polymer and the inorganic filler particles is (15-20):(4-6):(2-5).

4. The protective film layer according to claim 1, It is characterized in that The particle size of the inorganic filler particles is 10≤D90≤100nm; Preferably, the thickness of the protective film layer is 100nm to 1000nm; Preferably, the thickness of the protective film layer is 400nm-600nm.

5. A lithium electrode, It is characterized in that It comprises a lithium metal layer and a protective film layer coated on at least one side of the lithium metal layer, wherein the protective film layer is the protective film layer according to any one of claims 1 to 4.

6. The method for preparing a lithium electrode according to claim 5, It is characterized in that The steps include: Step S1, heating the first organic solvent to 40° C. to 80° C., then adding non-polar organic matter and polar polymer according to a ratio, and dissolving to obtain a mixed solution; Step S2, dispersing inorganic filler particles in the mixed solution according to a ratio to obtain a coating slurry; Step S3, coating the coating slurry on at least one side of the lithium metal layer, and obtaining the lithium electrode after drying; Wherein, the weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles and the first organic solvent is (10-25): (1-10): (0.5-5): (30-89).

7. The method for preparing a lithium electrode according to claim 6, It is characterized in that The first organic solvent is selected from at least one of toluene, xylene, tetrahydrofuran, carbon tetrachloride, and n-heptane; Preferably, in the step S1, after adding the non-polar organic matter and the polar polymer, stirring is performed for 1 h to 3 h to obtain the mixed solution.

8. The method for preparing a lithium electrode according to claim 6 or 7, It is characterized in that In the step S2, inorganic filler particles are added to the mixed solution, stirred for 2 hours to 5 hours, and then a second organic solvent is added and stirred for 20 minutes to 40 minutes to obtain the coating slurry; Preferably, the weight ratio of the non-polar organic matter, the polar polymer, the inorganic filler particles, the first organic solvent and the second organic solvent is (10-25): (1-10): (0.5-5): (30-45): (30-45); Preferably, the second organic solvent is selected from at least one of toluene, xylene, tetrahydrofuran, carbon tetrachloride, and n-heptane; Preferably, the coating slurry has a particle size of less than 500 nm.

9. The method for preparing a lithium electrode according to claim 6 or 7, It is characterized in that The coating method is selected from one of dip coating and roller coating; Preferably, the coating method is dip coating; More preferably, the coating speed of the dip coating is 2 mm / s to 20 mm / s, and further preferably the coating speed is 5 mm / s to 10 mm / s.

10. A lithium battery, It is characterized in that The lithium battery comprises the lithium electrode according to claim 5 or a lithium electrode prepared by the method for preparing a lithium electrode according to any one of claims 6 to 9.