Preparation method of boehmite composite material diaphragm capable of improving cycle performance of lithium battery
By grafting vinyltris(2-methoxyethoxy)silane onto the surface of a lithium-ion battery separator and coating it with boehmite slurry, the wettability and stability of the separator were improved, thereby enhancing the cycle performance and safety of the lithium battery.
Patent Information
- Application Number
- CN202411083777.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion battery separator materials have poor wettability to polar liquid electrolytes and low thermal stability, which affects cycle performance and safety performance.
A boehmite composite membrane was used, and the membrane performance was improved by grafting vinyltris(2-methoxyethoxy)silane onto the membrane surface and coating it with boehmite slurry.
It improves the ion transport capacity and separator stability of lithium batteries, reduces interface resistance and ohmic polarization, and enhances safety performance at high temperatures.
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical batteries, and in particular to a method for preparing a boehmite composite material diaphragm capable of improving the cycle performance of a lithium battery. Background Art
[0002] The past few decades have witnessed the rapid development of lithium-ion batteries (LIBs) for electronic digital devices and electric vehicles due to their high energy density, long cycle life, low self-discharge rate and environmental performance. The separator is an indispensable component in lithium-ion batteries, which not only completely isolates the cathode and anode, but also allows the free transfer of ions through the porous structure. At present, separator materials with excellent mechanical properties and superior electrochemical stability such as polyethylene (PE), polypropylene (PP), PP / PE / PP, etc. have been widely used in commercial LIBs. However, their inherent problems should not be ignored. The weak polarity of polyolefin separators leads to poor wettability to polar liquid electrolytes. In addition, the low thermal stability of polyolefins affects the safety performance at high temperatures and the cycle performance is poor. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a method for preparing a boehmite composite material separator that can improve the cycle performance of a lithium battery. The use of the boehmite composite material separator can improve the cycle performance of a lithium battery.
[0004] The technical solution of the present invention is achieved in this way: The present invention provides a method for preparing a boehmite composite material diaphragm capable of improving the cycle performance of a lithium battery, wherein the boehmite composite material diaphragm is used, and the preparation method of the diaphragm is as follows: S1: placing the diaphragm in a modifier solution and heating it to obtain a modified diaphragm; S2: coating the boehmite slurry on the modified diaphragm, and obtaining the boehmite composite diaphragm after drying.
[0005] Furthermore, the diaphragm material in step S1 is polymer PE.
[0006] Furthermore, the modifier in step S1 is vinyl tris (2-methoxyethoxy) silane.
[0007] Furthermore, the heating temperature in step S1 is 50-60°C.
[0008] Vinyl tri(2-methoxyethoxy)silane is grafted on the surface of the diaphragm to reduce the interface resistance and improve the ion transport capacity.
[0009] Non-volatile vinyl tris(2-methoxyethoxy)silane is relatively low cost, recyclable, easy to control, and convenient for large-scale application.
[0010] Furthermore, the preparation method of boehmite in step S2 is: S1: placing aluminum hydroxide in a ball milling jar and ball milling using a planetary ball mill; S2: The ball-milled aluminum hydroxide powder is placed in a crucible for first heating, and the first heating is heated from room temperature to 160-180° C.; S3: Perform the second stage of heating, the second stage of heating is heated from 160-180°C to 180-220°C, and stay at the end temperature of the reaction for 0.5-1h; S4: After the heating reaction is completed, cool to room temperature and collect the obtained white powder; S5: The collected white powder is sieved to remove magnetism, thereby obtaining the boehmite.
[0011] The method for preparing boehmite has the advantages of simple synthesis process, high safety, low requirements on equipment, low cost and excellent economy.
[0012] Furthermore, the boehmite slurry in step S2 further comprises a dispersant and a binder.
[0013] Furthermore, the binder accounts for 1-5wt% of the boehmite slurry.
[0014] Furthermore, the dispersant accounts for 1-5 wt % of the boehmite slurry.
[0015] The boehmite on the PE separator has good electrolyte affinity, avoids the formation of microbubbles, and reduces the pore structure of the PE framework, which plays a key role in improving the ionic conductivity of the separator and reducing the ohmic polarization at high current density.
[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. Vinyl tris(2-methoxyethoxy)silane grafted on the surface of the diaphragm can reduce the interface resistance and improve the ion transport capacity.
[0017] 2. Boehmite on the PE diaphragm improves ionic conductivity, reduces ohmic polarization and enhances the stability of the diaphragm. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Reagent Description: Aluminum hydroxide, vinyl tris(2-methoxyethoxy)silane, ethanol, polyvinylidene fluoride, fatty acid polyethylene glycol esters, analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0020] Preparation Example 1 S1: Select aluminum hydroxide powder commonly found in commerce as the reaction raw material, weigh 0.5 kg of aluminum hydroxide using an electronic balance, place it in a ball mill, and use a planetary ball mill for dry grinding at a ball mill speed of 400 rpm for 2 hours; S2: The ball-milled aluminum hydroxide powder is placed in a reaction crucible and subjected to a first two-stage heating reaction: the first stage heating program is set to heat from 30°C to 170°C at a heating rate of 5°C / min, and nitrogen is continuously introduced during the reaction; S3: The second heating program is set to heat from 170°C to 190°C, with a heating rate of 10°C / min. Nitrogen is continuously introduced during the reaction, and the end temperature is 190°C for 0.5h. S4: After the reaction is completed, the mixture is cooled to room temperature and the resulting white powder is collected as the final product; S5: The collected white powder is sieved to remove magnetism to obtain the final product. Example 1
[0021] S1: Vinyltri(2-methoxyethoxy)silane was dissolved in ethanol to prepare a 10 wt% homogeneous solution, and then the membrane was placed in the solution and irradiated at 60 kGy at 55° C. for 2 h.
[0022] S2: Dissolve the boehmite of Preparation Example 1 in acetone to prepare a 20wt% homogeneous solution, add 3wt% of the solution mass of the adhesive polyvinylidene fluoride and 3wt% of the solution mass of the dispersant fatty acid polyethylene glycol ester and stir evenly. Use a scraper coating method to coat the boehmite slurry on one side of the PE diaphragm, and the coating thickness is about 3μm. Transfer the coated diaphragm to a constant temperature blast drying oven at 60°C to remove excess moisture on the surface, and then place it in a vacuum drying oven at 50°C to dry for 12h to remove moisture in the pores, and the surface coated modified diaphragm can be obtained. Example 2
[0023] The difference between this embodiment and embodiment 1 is that the mass fraction of the vinyl tris(2-methoxyethoxy)silane solution in step S1 is 5 wt %.
[0024] The other parts are exactly the same as those in Example 1. Example 3
[0025] The difference between this embodiment and embodiment 1 is that the mass fraction of the vinyl tris(2-methoxyethoxy)silane solution in step S1 is 20 wt %.
[0026] The other parts are exactly the same as those in Example 1. Example 4
[0027] The difference between this embodiment and embodiment 1 is that the heating temperature in step S1 is 50°C.
[0028] The other parts are exactly the same as those in Example 1. Example 5
[0029] The difference between this embodiment and embodiment 1 is that the heating temperature in step S1 is 60°C.
[0030] The other parts are exactly the same as those in Example 1.
[0031] Comparative Example 1 The difference between this comparative example and Example 1 is that vinyl tris(2-methoxyethoxy)silane is not added in step S1.
[0032] The other parts are exactly the same as those in Example 1.
[0033] Comparative Example 2 The difference between this comparative example and Example 1 is that boehmite is not added in step S1.
[0034] The other parts are exactly the same as those in Example 1.
[0035] Tests and Results After the assembled LiFePO4 / diaphragm / Li battery was cycled for 1000 times at 1C in the voltage range of 2.4~4.2V, its discharge specific capacity was tested to determine its cycle stability.
[0036] The results are shown in Table 1 Table 1 project Capacity retention rate (%) Example 1 80 Example 2 75 Example 3 84 Example 4 73 Example 5 78 Comparative Example 1 65 Comparative Example 2 45 It can be seen from Examples 1-3 and Comparative Example 1 in Table 1 that with the addition of vinyltri(2-methoxyethoxy)silane, the cycle stability of the diaphragm is improved.
[0037] It can be seen from Examples 1, 4-5 in Table 1 that temperature affects the grafting of vinyl tris(2-methoxyethoxy)silane onto the diaphragm. When the temperature is low, the bonding is insufficient, but when the temperature is high, the stability of the diaphragm is affected, causing it to shrink.
[0038] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery, characterized in that: The preparation method of the diaphragm is: S1: placing the diaphragm in a modifier solution and heating it to obtain a modified diaphragm; S2: coating the boehmite slurry on the modified diaphragm, and obtaining the boehmite composite diaphragm after drying.
2. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 1, characterized in that: The diaphragm material in step S1 is polymer PE.
3. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 1, characterized in that: The modifier in step S1 is vinyl tris (2-methoxyethoxy) silane.
4. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 1, characterized in that: The heating temperature in step S1 is 50-60°C.
5. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 1, characterized in that: The preparation method of boehmite in step S2 is: S1: placing aluminum hydroxide in a ball milling jar and ball milling it using a planetary ball mill; S2: The ball-milled aluminum hydroxide powder is placed in a crucible for first heating, and the first heating is heated from room temperature to 160-180°C; S3: Perform the second stage of heating, the second stage of heating is heated from 160-180°C to 180-220°C, and stay at the end temperature of the reaction for 0.5-1h; S4: After the heating reaction is completed, cool to room temperature and collect the obtained white powder; S5: The collected white powder is sieved to remove magnetism, thereby obtaining the boehmite.
6. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 1, characterized in that: The boehmite slurry in step S2 further comprises a dispersant and a binder.
7. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 5, characterized in that: The binder accounts for 1-5 wt % of the boehmite slurry.
8. The method for preparing a boehmite composite material separator capable of improving the cycle performance of a lithium battery according to claim 5, characterized in that: The dispersant accounts for 1-5 wt % of the boehmite slurry.
Citation Information
Patent Citations
Preparation method of ceramic grafted diaphragm and application of ceramic grafted diaphragm in lithium battery
CN104600229A
Radiating modification lithium ion battery diaphragm and preparation method thereof
CN104882581A
Waterborne ceramic coated membrane for lithium ion battery and preparation method thereof
CN105789539A
Ceramic slurry for lithium battery separator and preparation method and application method of ceramic slurry
CN106531941A
Production process of lithium battery separator
CN106684293A