Surface coated cutting tool

By adjusting the element proportion and structure in the composite carbon nitride layer of the coating tool, combined with the design of the lower and upper layers, the two opposite relationship between hardness and toughness of the coating tool is solved, and the thermal stability at high temperatures is improved and oxidation resistance, achieving longer wear resistance.

CN119053397AActive Publication Date: 2024-11-29MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380029558.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-15
Publication Date
2024-11-29
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

Existing coating tools are difficult to take into account high hardness and high toughness, especially in terms of thermal stability and oxidation resistance at high temperatures.

Method used

A composite carbon nitride layer is used, specifically composed of (TiVZrNb) or (TiVZrNbHfTa). By adjusting the atomic proportion and structure, a NaCl-shaped face-centered cubic structure is formed, the mixing entropy is increased to improve hardness and toughness, and an appropriate lower part is set on the surface of the matrix. and upper layer for enhanced durability.

Benefits of technology

The high hardness and toughness of the cladding are achieved, the thermal stability and oxidation resistance are improved, the service life of the tool is extended, and the wear resistance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053397A_ABST
    Figure CN119053397A_ABST
Patent Text Reader

Abstract

A surface-coated cutting tool having a coating layer, the coating layer having a composite carbonitride layer having an average thickness of 1.0 [mu] m or more and 20.0 [mu] m or less, the composite carbonitride layer containing Ti, V, Zr, and Nb at respective atomic ratios a1, a2, a3, and a4 of the metal components when the total atomic ratios of the metal components of the composite carbonitride layer are 1, the composite carbonitride layer contains non-metallic components C and N at the atomic ratios b1 and b2 of the non-metallic components, respectively, when the total of the atomic ratios of the non-metallic components of the composite carbonitride layer is 1, the composite carbonitride layer further contains unavoidable impurities, and a1, a2, a3, a4, b1 and b2 satisfy 0.01 < = a1 < = 0.60, 0.01 < = a2 < = 0.60, 0.01 < = a3 < = 0.60, 0.01 < = a4 < = 0.60, 0.20 < = b1 < = 0.80, 0.20 < = b2 < = 0.80, and Sconfig > = 0.80 R (R is a gas constant and ln is a natural logarithm); the composite carbonitride layer comprises crystal grains with a NaCl type face-centered cubic structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface-coated cutting tool (hereinafter, sometimes referred to as a coated tool). This application claims priority based on Japanese patent application No. 2022-55518 filed on March 30, 2022. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art

[0002] A coated tool having a coating layer formed on the surface of a substrate such as tungsten carbide (hereinafter referred to as WC)-based cemented carbide is known, and it is known that the coated tool exhibits excellent wear resistance.

[0003] Furthermore, in order to enhance the durability of the coated tool, various proposals have been made regarding improvements to the coating layer.

[0004] For example, Patent Document 1 describes a coated tool having a substrate and a coating layer on the substrate, wherein the coating layer is a face-centered cubic structure (Ti) having a lattice constant of 0.403 to 0.455 nm. x Zr 1-x )(C y N 1-y )(0.4<x<0.95, 0.2<y<0.9) or a face-centered cubic structure (Ti) with a lattice constant of 0.430~0.450nm x Hf 1-x )(C y N 1-y )(0.4<x<0.95, 0.2<y<0.9), the coating layer is relatively hard and has wear resistance.

[0005] In addition, for example, Patent Document 2 describes a coated tool (insert blade) in which a base body is coated with Ti having an fcc structure with a lattice constant of 0.427 to 0.453 nm. 1-x Me x The nitride (0.1≤x≤0.9, Me is one or more of Zr and Hf) of the coated tool has a harder coating layer and is suitable for dry cutting of stainless steel.

[0006] Patent Document 1: Japanese Patent No. 4028891

[0007] Patent Document 2: U.S. Patent Application Publication No. 2016 / 0298233 Summary of the invention

[0008] The present invention has been made in view of the above circumstances and the above solutions, and an object of the present invention is to provide a coated tool having a coating layer having high hardness and improved toughness.

[0009] A surface-coated cutting tool according to an embodiment of the present invention is characterized in that:

[0010] having a substrate and a coating layer on a surface of the substrate,

[0011] The coating layer comprises a composite carbonitride layer,

[0012] The average thickness of the composite carbonitride layer is 1.0 μm or more and 20.0 μm or less,

[0013] When the total atomic ratio of the metal components in the composite carbonitride layer is 1, the metal components Ti, V, Zr, and Nb are contained at atomic ratios a1, a2, a3, and a4 of the metal components, respectively.

[0014] When the total atomic ratio of the non-metallic components in the composite carbonitride layer is 1, the non-metallic components C and N are contained at atomic ratios b1 and b2 of the non-metallic components, respectively.

[0015] The composite carbonitride layer further contains inevitable impurities,

[0016] The a1, a2, a3, a4, b1, and b2 are as follows:

[0017] 0.01≤a1≤0.60

[0018] 0.01≤a2≤0.60

[0019] 0.01≤a3≤0.60

[0020] 0.01≤a4≤0.60

[0021] 0.20≤b1≤0.80

[0022] 0.20≤b2≤0.80,

[0023] When n=4 and m=2, S is expressed by Formula 1 (where ln in Formula 1 is a natural logarithm). config is 0.80R (R is the gas constant) or more,

[0024] The composite carbonitride layer comprises grains having a NaCl-type face-centered cubic structure,

[0025]

[0026] Furthermore, the surface-coated cutting tool according to the above-mentioned embodiment may satisfy at least one of the following items (1) and (2).

[0027] (1) The composite carbonitride layer further contains at least one of Hf and Ta as the metal component, and the atomic ratios of Hf and Ta are a5 and a6, respectively.

[0028] The a5 and a6 are as follows:

[0029] a5<0.01

[0030] a6<0.01,

[0031] When n=6 and m=2, S represented by Formula 1 config (Among them, when a i When (i=5 or 6) is zero (not included), a i ln(a i )=0) is 0.80R or more.

[0032] (2) The composite carbonitride layer contains 0.50 atomic % or less of Cl.

[0033] The coating layer of the surface-coated cutting tool has high hardness and high toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram showing the crystal structure of TiN.

[0035] Figure 2 Schematic diagram showing the crystal structure of (TiVZrNb)(CN) or (TiVZrNbHfTa)(CN). DETAILED DESCRIPTION

[0036] The coating layer of the surface-coated cutting tool has a contradictory relationship between high hardness and high toughness, and it is considered difficult to achieve both in the conventional solid solution strengthening theory.

[0037] On the other hand, in recent years, although research has been conducted on solid solutions that increase the mixing entropy of alloys such as high entropy alloys, which are alloys formed by mixing five or more elements in approximately equal atomic ratios, and multi principal element alloys, which are alloys composed of three or more elements and at least two or more main elements, there has been no research on increasing the mixing entropy of the coating layer of the coated tool.

[0038] The present inventors have conducted intensive research on the solid solution (alloy) constituting the coating layer of the coated tool in order to achieve both high hardness and high toughness, which are in a contradictory relationship and cannot be achieved by conventional coating layers, by increasing the mixing entropy.

[0039] The results yielded the following insights:

[0040] If the mixing entropy is increased in the composite carbonitride layer of a specific composition constituting the coating layer of the coated tool,

[0041] (i) The composite carbonitride layer with a specific composition is composed of multiple atoms with different atomic radii, which causes distortion in the grains, and improves hardness and toughness.

[0042] (ii) The thermal stability and oxidation resistance of the composite carbonitride layer at high temperatures are improved.

[0043] Next, a surface-coated cutting tool according to an embodiment of the present invention will be described.

[0044] In addition, in the present specification and claims, when "L~M" (L and M are both numerical values) is used to express a numerical range, it has the same meaning as "above L and below M", and the range includes an upper limit M and a lower limit L. When only the upper limit is recorded in terms of unit, the units of the upper limit M and the lower limit L are the same.

[0045] I. First Implementation

[0046] The composite carbonitride of (TiVZrNb) (may be expressed as (TiVZrNb)(CN)) constituting the coating layer according to the first embodiment will be described.

[0047] 1. Coating layer

[0048] 1-1, (TiVZrNb)(CN) layer

[0049] (1) Crystal structure

[0050] (TiVZrNb)(CN) is Figure 2 That is, any one of the Ti, V, Zr and Nb atoms with different atomic radii is present at the cation site 4, and the C and N atoms are randomly mixed at the anion sites 2 and 3, respectively, to form a lattice. This lattice is similar to that in Figure 1 Compared to the crystal structure of TiN (Ti atom 1, N atom 2) schematically shown in FIG, each atom is displaced from the ideal lattice point position. As a result, distortion occurs in the lattice (in Figure 2 The hardness and toughness will be improved due to the distortion. Figure 2 The displacement of each atom is also schematically shown in FIG.

[0051] (2) Average thickness

[0052] The average thickness of the composite carbonitride layer, i.e., the (TiVZrNb)(CN) layer, is preferably 1.0 μm or more and 20.0 μm or less. The reason is that if the average thickness is less than 1.0 μm, the average thickness of the (TiVZrNb)(CN) layer is thin, and therefore the durability cannot be fully ensured. On the other hand, if the average thickness is greater than 20.0 μm, the grains of the (TiVZrNb)(CN) layer are easily coarsened, and chipping is easily caused. The average thickness of the (TiVZrNb)(CN) layer is more preferably 3.0 μm or more and 16.0 μm or less.

[0053] (3) Composition

[0054] In the formula: (Ti a1 V a2 Zr a3 Nb a4 )(C b1 N b2 ) represents the composition of the composite carbonitride layer, i.e., the (TiVZrNb)(CN) layer,

[0055] Preferably, a1, a2, a3, a4, b1, and b2 are a1+a2+a3+a4=1, b1+b2=1.

[0056] And a1, a2, a3, a4, b1, b2 are as follows:

[0057] 0.01≤a1≤0.60

[0058] 0.01≤a2≤0.60

[0059] 0.01≤a3≤0.60

[0060] 0.01≤a4≤0.60

[0061] 0.20≤b1≤0.80

[0062] 0.20≤b2≤0.80,

[0063] When n=4 and m=2, S is expressed by Formula 1 (where ln in Formula 1 is a natural logarithm). config It is greater than 0.80R (R is the gas constant).

[0064] Furthermore, unintentional and inevitable impurities mixed in during the production process may be contained.

[0065]

[0066] When the values ​​of a1, a2, a3, a4, b1 and b2 satisfy the above relationship, the mixing entropy of the (TiVZrNb)(CN) layer is increased, and the (TiVZrNb)(CN) layer has the physical properties (i) to (ii) obtained from the above findings.

[0067] And, preferably S config A1, a2, a3, a4, b1, b2 are determined in a larger way. config The calculated upper limit value is 1.04R.

[0068] (4) Cl content

[0069] If the film is formed by a CVD method using chloride as a raw material gas, it is inevitable to contain a very small amount of Cl (the amount of which can be confirmed by single element analysis of chlorine alone). And if the Cl content is 0.50 atomic % or less, the (TiVZrNb)(CN) layer has lubricity due to Cl.

[0070] Here, the Cl content (atomic %) is the ratio of Cl to all atoms of Ti, V, Zr, Nb, C, N, and Cl.

[0071] (5) NaCl-type face-centered cubic structure

[0072] The (TiVZrNb)(CN) layer preferably has grains of a NaCl-type face-centered cubic structure. However, it may contain grains other than the NaCl-type face-centered cubic structure, and the presence of grains other than the NaCl-type face-centered cubic structure is unintentional. In the claims and this specification, grains having a NaCl-type face-centered cubic structure mean that, in addition to grains of the NaCl-type face-centered cubic structure, there may also be grains of the unintentional NaCl-type face-centered cubic structure.

[0073] 1-2. Other layers

[0074] (1) Lower layer

[0075] A lower layer may be provided between the substrate and the (TiVZrNb)(CN) layer, the lower layer being composed of one or more Ti compound layers (not limited to stoichiometric composition) selected from among a Ti nitride layer, a carbide layer, and a carbonitride layer, and the total average thickness of the lower layer is 0.1 to 20.0 μm. If the lower layer is provided, the adhesion between the substrate and the (TiVZrNb)(CN) layer is improved.

[0076] (2) Upper layer

[0077] An upper layer may be provided on the upper portion of the (TiVZrNb)(CN) layer, the upper layer being composed of a Ti compound (not limited to the stoichiometric composition) layer and / or an aluminum oxide (not limited to the stoichiometric composition) layer of one or more of a Ti nitride layer, a carbide layer, a carbonitride layer, and an oxide layer, and the total average thickness of the upper layer is 0.1 to 25.0 μm. If the upper layer is provided, chipping resistance and wear resistance are improved.

[0078] (3) Unintentionally generated layers

[0079] When the gas pressure or temperature in the CVD furnace becomes unstable, a layer different from the (TiVZrNb)(CN) layer, the lower layer, and the upper layer may be formed unintentionally.

[0080] 2. Matrix

[0081] (1) Material

[0082] If the material is a material of a conventionally known matrix, any material may be used as long as it does not hinder the achievement of the purpose of the present invention. For example, the material is any one of WC-based cemented carbide (in addition to WC, it also includes Co, and further includes an alloy formed by adding carbides or nitrides of Ti, Zr, Ta, Nb, Cr, etc.), cermet (ceramics with TiC, TiN, TiCN, etc. as the main component), ceramic (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide), and cBN sintered body.

[0083] (2) Shape

[0084] The shape of the base body is not particularly limited as long as it is a shape used as a cutting tool, and examples thereof include the shape of an insert and the shape of a whole tool.

[0085] 3. Determination method

[0086] The average thickness, the content of each element, and the average chlorine content of the (TiVZrNb)(CN) layer of the present embodiment were determined as follows.

[0087] (1) Average thickness

[0088] The average thickness of the (TiVZrNb)(CN) layer etc. can be obtained as follows. A sample for observing the longitudinal section of the coating layer is prepared using a cross-section polisher (CP) or the like, and the longitudinal section is observed using a scanning electron microscope (SEM). The thickness of the layer at multiple locations (e.g., five locations) is measured, and their average value is taken as the average thickness of the (TiVZrNb)(CN) layer etc. In addition, the definition of the surface of the substrate will be described later.

[0089] Here, the longitudinal section refers to a section perpendicular to the surface of the base body when the surface of the base body is treated as a flat surface by ignoring minute irregularities on the surface of the base body in the insert.

[0090] The surface of the substrate refers to an average line (straight line) of the interface roughness between the substrate and the coating layer in the observed image of the longitudinal section.

[0091] That is, based on the observed image of the longitudinal section, the interface between the coating layer (if there is a lower layer, the lower layer is used instead of the (TiVZrNb)(CN) layer) and the substrate is determined, and the average line is drawn for the obtained roughness curve of the interface between the coating layer and the substrate, and the average line is used as the surface of the substrate. In addition, the direction perpendicular to the average line is set as the direction perpendicular to the substrate (the thickness direction of the layer).

[0092] Even when the substrate has a curved surface, if the radius of curvature of the curved surface is sufficiently large relative to the thickness of the coating, the surface of the substrate can be determined by the same method because the interface between the coating and the substrate in the measurement area is approximately flat.

[0093] (2) Content of each element and chlorine content in the coating layer

[0094] The contents of each element and the chlorine content in the (TiVZrNb)(CN) layer were determined as follows.

[0095] Regarding the contents a1, a2, a3, a4 of Ti, V, Zr, and Nb, the contents b1, b2 of C and N, and the chlorine content, an electron probe micro analyzer (EPMA) was used. In the sample whose surface was polished, electron beams were irradiated from the surface side of the sample, and the average value of the analysis results of 10 characteristic X-rays was obtained.

[0096] (3) Identification of the crystal structure of the (TiVZrNb)(CN) layer

[0097] The (TiVZrNb)(CN) layer was subjected to an X-ray diffraction test using an X-ray diffraction device, and it was confirmed that the layer had a NaCl-type face-centered cubic structure. In addition, the X-ray diffraction was measured by a 2θ-θ method using CuKα rays, and the measurement conditions were as follows: a measurement range (2θ): 15 to 135 degrees, an X-ray output: 45 kV, 40 mA, a divergence slit: 0.5 degrees, and a scanning step length: 0.013 degrees.

[0098] 4. Manufacturing method

[0099] Regarding the method for manufacturing the (TiVZrNb)(CN) layer of the present embodiment, for example, it can be carried out by a CVD method using gases such as TiCl4, ZrCl4, VCl4, NbCl5, H2, HCl, N2, CH3CN, Ar, and H2.

[0100] II. Second Implementation

[0101] The composite carbonitride of (TiVZrNbHfTa) (may be expressed as (TiVZrNbHfTa)(CN)) constituting the coating layer according to the second embodiment will be described.

[0102] 1. Coating layer

[0103] 1-1, (TiVZrNbHfTa)(CN) layer

[0104] (1) Crystal structure

[0105] The crystal structure is the structure when "(TiVZrNb)(CN)" and "Ti, V, Zr, Nb atoms" in the description related to the crystal structure of the aforementioned first embodiment are replaced by "(TiVZrNbHfTa)(CN)" and "Ti, V, Zr, Nb, Hf, Ta atoms (Hf and Ta are selected according to the composition)", respectively.

[0106] (2) Average thickness

[0107] The average thickness is the thickness obtained by replacing "(TiVZrNb)" with "(TiVZrNbHfTa)" in the description of the average thickness in the first embodiment.

[0108] (3) Composition

[0109] In the formula: (Ti a1 V a2 Zr a3 Nb a4 Hf a5 Ta a6 )(C b1 N b2 ) represents the composition of the composite carbonitride layer, i.e., the (TiVZrNbHfTa)(CN) layer,

[0110] Preferably, a1, a2, a3, a4, a5, a6, b1, and b2 are a1+a2+a3+a4+a5+a6=1, b1+b2=1, and a1, a2, a3, a4, a5, a6, b1, and b2 are as follows:

[0111] 0.01≤a1≤0.60

[0112] 0.01≤a2≤0.60

[0113] 0.01≤a3≤0.60

[0114] 0.01≤a4≤0.60

[0115] 0.00≤a5<0.01

[0116] 0.00≤a6<0.01

[0117] 0.20≤b1≤0.80

[0118] 0.20≤b2≤0.80,

[0119] When n=6 and m=2, S is expressed by Formula 1 (where ln in Formula 1 is a natural logarithm). config It is greater than 0.80R (R is the gas constant).

[0120] Furthermore, unintentional and inevitable impurities mixed in during the production process may be contained.

[0121]

[0122] Here, when a i When (i=5 or 6) is 0.00 (when Hf or Ta is not contained), a i ln(a i ) is treated as 0 (zero).

[0123] When the values ​​of a1, a2, a3, a4, a5, a6, b1 and b2 satisfy the above relationship, the mixing entropy of the (TiVZrNbHfTa)(CN) layer will increase, and the (TiVZrNbHfTa)(CN) layer will have the physical properties (i) to (ii) obtained in the above-mentioned insights.

[0124] And, preferably S config A larger way to determine a1, a2, a3, a4, a5, a6, b1, b2.

[0125] Since the upper limits of a5 and a6 are both less than 0.01, S config The calculation upper limit is 1.08R.

[0126] (4) Cl content

[0127] The Cl content is the content when "(TiVZrNb)(CN)" is replaced with "(TiVZrNbHfTa)(CN)" in the description of the Cl content in the first embodiment. That is, the Cl content (atomic %) is the ratio of Cl to all atoms of Ti, V, Zr, Nb, Hf, Ta, C, N, and Cl.

[0128] (5) NaCl-type face-centered cubic structure

[0129] The NaCl type face-centered cubic structure is a structure obtained by replacing "(TiVZrNb)" with "(TiVZrNbHfTa)" in the description of the NaCl type face-centered cubic structure in the first embodiment.

[0130] 1-2. Other layers

[0131] The other layers are layers obtained by replacing "(TiVZrNb)" with "(TiVZrNbHfTa)" in the description of the other layers in the first embodiment.

[0132] 2. Substrate

[0133] The substrate is the same as that described in the first embodiment.

[0134] 3. Determination method

[0135] The measurement method is the same as that in the description of the measurement method in the first embodiment above, except that "(TiVZrNb)" is replaced with "(TiVZrNbHfTa)". The contents of Hf and Ta are also measured by EPMA.

[0136] 4. Manufacturing method

[0137] The manufacturing method of the (TiVZrNbHfTa) (CN) layer of the present embodiment can be carried out by, for example, using a gas obtained by adding HfCl4 and TaCl5 to the film-forming gas of the first embodiment (i.e., gases of TiCl4, ZrCl4, VCl4, NbCl5, HfCl4, TaCl5, H2, HCl, N2, CH3CN, Ar, and H2).

[0138] The above description includes the following additional features.

[0139] (Note 1)

[0140] A surface-coated cutting tool comprises a substrate and a coating layer on the surface of the substrate, characterized in that:

[0141] The coating layer comprises a composite carbonitride layer,

[0142] The average thickness of the composite carbonitride layer is 1.0 μm or more and 20.0 μm or less,

[0143] When the total atomic ratio of the metal components in the composite carbonitride layer is 1, the metal components Ti, V, Zr, and Nb are contained at atomic ratios a1, a2, a3, and a4 of the metal components, respectively.

[0144] When the total atomic ratio of the non-metallic components in the composite carbonitride layer is 1, the non-metallic components C and N are contained at atomic ratios b1 and b2 of the non-metallic components, respectively.

[0145] The composite carbonitride layer further contains inevitable impurities,

[0146] The a1, a2, a3, a4, b1, and b2 are as follows:

[0147] 0.01≤a1≤0.60

[0148] 0.01≤a2≤0.60

[0149] 0.01≤a3≤0.60

[0150] 0.01≤a4≤0.60

[0151] 0.20≤b1≤0.80

[0152] 0.20≤b2≤0.80,

[0153] When n=4 and m=2, S is expressed by Formula 1 (where ln in Formula 1 is a natural logarithm). config is 0.80R (R is the gas constant) or more,

[0154] The composite carbonitride layer comprises grains having a NaCl-type face-centered cubic structure,

[0155]

[0156] (Note 2)

[0157] The surface coated cutting tool according to Supplementary Note 1 is characterized in that:

[0158] The composite carbonitride layer further contains at least one of Hf and Ta as the metal component, and the atomic ratios of Hf and Ta are a5 and a6, respectively.

[0159] The a5 and a6 are as follows:

[0160] a5<0.01

[0161] a6<0.01,

[0162] When n=6 and m=2, S represented by Formula 1 config (Among them, when a i When (i=5 or 6) is zero (not included), a i ln(a i )=0) is 0.80R or more.

[0163] (Note 3)

[0164] The surface-coated cutting tool according to Supplement 1 or 2 is characterized in that the composite carbonitride layer contains less than 0.50 atomic % of Cl.

[0165] (Note 4)

[0166] A surface-coated cutting tool according to any one of Notes 1 to 3, characterized in that there is a lower layer between the substrate and the composite carbonitride layer, the lower layer being composed of one or more Ti compound layers among a Ti nitride layer, a carbide layer and a carbonitride layer, and the total average thickness of the lower layer is 0.1 to 20.0 μm.

[0167] (Note 5)

[0168] A surface-coated cutting tool according to any one of Notes 1 to 4, characterized in that an upper layer is provided on the upper part of the composite carbonitride layer, the upper layer being composed of one or more Ti compound layers selected from the group consisting of a Ti nitride layer, a carbide layer, a carbonitride layer and an oxide layer, and the total average thickness of the upper layer is 0.1 to 25.0 μm.

[0169] Example

[0170] The present invention is not limited to the embodiments. That is, although a cutting tool with a blade using WC-based cemented carbide as a substrate is listed, the material of the substrate can be any of the aforementioned materials, and the shape can also be other shapes such as a whole tool as described above.

[0171] <Example of the first embodiment>

[0172] 1. Manufacturing of substrate

[0173] As raw material powders, WC powder, TiC powder, ZrC powder, TaC powder, NbC powder, Cr3C2 powder, TiN powder and Co powder were prepared, and these raw material powders were blended according to the composition shown in Table 1, and wax was further added and wet-mixed in acetone using a ball mill for 24 hours. After drying under reduced pressure, the powders were pressed at a pressure of 98 MPa into a compact of a specified shape.

[0174] Then, the green compact was vacuum sintered, and after sintering, the cutting edge portion was ball-milled to an R of 0.05 mm to produce WC-based cemented carbide substrates A to C having a blade shape of CNMG120408-MA manufactured by Mitsubishi Materials Corporation.

[0175] 2. Film formation

[0176] On the surfaces of substrates A to C, (TiVZrNb)(CN) layers were formed using a CVD apparatus to obtain Examples 1 to 10 shown in Table 5. The film formation conditions were as shown in Table 2, but were roughly as follows.

[0177] Reaction gas composition (gas content is volume %):

[0178] TiCl4: 0.02~0.10%

[0179] ZrCl4: 0.10~0.50%

[0180] VCl4: 0.02~0.10%

[0181] NbCl5: 0.02~0.10%

[0182] CH3CN: 0.10~0.50%

[0183] HCl: 0.10~0.50%

[0184] N2: 0.0~12.0%

[0185] Ar: 10.0~50.0%

[0186] H2: Remaining

[0187] Reaction atmosphere pressure: 4.5~12.0kPa

[0188] Reaction atmosphere temperature: 800~950℃

[0189] In addition, regarding Examples 3 to 10, the lower layer and / or upper layer shown in Table 4 were formed under the conditions shown in Table 3.

[0190] For comparison, (TiVZrNb)(CN) layers were formed on the surfaces of substrates A to C according to the film forming conditions shown in Table 2, and Comparative Examples 1 to 10 shown in Table 5 were obtained.

[0191] Regarding the production process of the comparative example, the composition of the raw material gas is different from that of the working example.

[0192] In addition, regarding Comparative Examples 3 to 10, the lower layer and / or upper layer shown in Table 4 were formed under the conditions shown in Table 3.

[0193] Furthermore, for comparison with the prior art, TiCN layers and lower layers, lower layers and upper layers shown in Table 4 were formed on the surfaces of substrates A and C under the conditions shown in Table 3 to produce prior art examples 1 to 2 shown in Table 5.

[0194] Regarding the above-mentioned Examples 1 to 10, Comparative Examples 1 to 10 and Conventional Examples 1 to 2, the average thickness of each layer, the content of each element, the chlorine content, and whether or not the layer had a NaCl-type face-centered cubic structure were measured using the above-mentioned method.

[0195] These results are summarized in Table 5.

[0196] [Table 1]

[0197]

[0198] [Table 2]

[0199]

[0200] [Table 3]

[0201]

[0202] [Table 4]

[0203]

[0204] [Table 5]

[0205]

[0206] In Table 5, since the conventional examples 1 and 2 do not contain V, Zr, and Nb, S config It is the result calculated by -R / 2[b1ln(b1)+b2ln(b2)].

[0207] “**” indicates a content below the quantitative accuracy of the analyzer, indicating that a peak of the characteristic X-ray spectrum of chlorine was confirmed by single element detection analysis of chlorine alone, and that a trace amount of chlorine was confirmed to be contained.

[0208] In addition, it was confirmed that all of the examples, comparative examples, and conventional examples substantially had crystal grains of a NaCl-type face-centered cubic structure.

[0209] Next, regarding Examples 1 to 10, Comparative Examples 1 to 10 and Existing Examples 1 to 2, a wet end face cutting test was carried out on a hollow round bar with two grooves at equal intervals made of alloy steel SCM440, all of which were threadedly fastened to the front end of a tool steel turning tool with a fixing fixture, and the wear width of the flank of the cutting edge was measured.

[0210] Since this cutting test is a process in which flank wear is likely to progress and includes intermittent processing, the blade tip is likely to chip. Therefore, since this cutting test is a process requiring both wear resistance and chipping resistance, it is suitable for evaluating hardness and toughness.

[0211] Cutting test

[0212] Workpiece: JIS·SCM440

[0213] Hollow round rod with two slots (20mm wide) at equal intervals

[0214] (Outer diameter Φ180, inner diameter Φ50)

[0215] Cutting speed: 250m / min

[0216] Cutting depth: 1.5mm

[0217] Feed rate: 0.4mm / rev.

[0218] Cutting times: 20 times

[0219] The results of the cutting test are shown in Table 6. In addition, for Comparative Examples 1 to 10 and Conventional Examples 1 to 2, the life was reached before the number of cutting passes reached 20 due to chipping or flank wear (life judgment criterion: flank wear width 0.4 mm), so the number of cutting passes to reach this life is shown.

[0220] [Table 6]

[0221]

[0222] From the results shown in Table 6, it can be seen that Examples 1 to 10 have less wear, no chipping occurs, and both hardness and toughness are improved, thereby exhibiting excellent cutting performance for a long time.

[0223] In contrast, the amounts of wear in Comparative Examples 1 to 10 and Conventional Examples 1 to 2 were large or chipping occurred, and the service life was reached in a short time.

[0224] <Example of Second Embodiment>

[0225] 1. Manufacturing of substrate

[0226] WC-based cemented carbide substrates A to C having the same insert shape as that of CNMG120408-MA manufactured by Mitsubishi Materials Corporation as that of the first embodiment were produced.

[0227] 2. Film formation

[0228] On the surfaces of substrates A to C, (TiVZrNbHfTa)(CN) layers were formed using a CVD apparatus to obtain Examples 11 to 15 shown in Table 9. The film formation conditions were as shown in Table 7, but were roughly as follows.

[0229] Reaction gas composition (gas content is volume %):

[0230] TiCl4: 0.02~0.10%

[0231] VCl4: 0.02~0.10%

[0232] ZrCl4: 0.10~0.50%

[0233] NbCl5: 0.02~0.10%

[0234] *HfCl4: 0.00~0.02%

[0235] *TaCl5: 0.00~0.01%

[0236] CH3CN: 0.10~0.50%

[0237] HCl: 0.10~0.50%

[0238] N2: 0.0~12.0%

[0239] Ar: 10.0~50.0%

[0240] H2: Remaining

[0241] *HfCl4 and *TaCl5 are selected according to the composition of the (TiVZrNbHfTa)(CN) layer.

[0242] Reaction atmosphere pressure: 4.5~12.0kPa

[0243] Reaction atmosphere temperature: 800~950℃

[0244] In addition, regarding Examples 13 to 15, the lower layer and / or upper layer shown in Table 8 were formed under the conditions shown in Table 3.

[0245] For comparison, (TiVZrNbHfTa)(CN) layers were formed on the surfaces of substrates A to C according to the film forming conditions shown in Table 7, and Comparative Examples 11 to 15 shown in Table 9 were obtained.

[0246] In the manufacturing process of the comparative example, the composition of the raw material gas is different from that of the working example.

[0247] In addition, regarding Comparative Examples 13 to 15, the lower layer and / or upper layer shown in Table 8 were formed under the conditions shown in Table 3.

[0248] For the above-mentioned Examples 11 to 15 and Comparative Examples 11 to 15, the average thickness of each layer, the content of each element, the chlorine content, and whether or not the layer had a NaCl-type face-centered cubic structure were measured using the above-mentioned method. These results are summarized in Table 9.

[0249] [Table 7]

[0250]

[0251] [Table 8]

[0252]

[0253] [Table 9]

[0254]

[0255] In Table 9, "**" indicates that the content was below the quantitative accuracy of the analyzer, and therefore, a peak of the characteristic X-ray spectrum of chlorine was confirmed by single element detection analysis of chlorine alone, and a trace amount of chlorine was confirmed.

[0256] In addition, it was confirmed that all of the Examples, Comparative Examples, and Conventional Examples had crystal grains of a NaCl-type face-centered cubic structure.

[0257] Next, for Examples 11 to 15 and Comparative Examples 11 to 15, a wet end face cutting test was carried out on a hollow round bar with two grooves at equal intervals made of alloy steel SCM440, while the front end portion of the tool steel turning tool was tightened to the front end portion of the tool steel turning tool with a fixing fixture, and the wear width of the back face of the cutting edge was measured.

[0258] Since this cutting test is a process in which flank wear is likely to progress and includes intermittent processing, the blade tip is likely to chip. Therefore, since this cutting test is a process requiring both wear resistance and chipping resistance, it is suitable for evaluating hardness and toughness.

[0259] Cutting test

[0260] Workpiece: JIS·SCM440

[0261] A hollow round rod with two slots (20 mm wide) at equal intervals

[0262] (Outer diameter Φ180, inner diameter Φ50)

[0263] Cutting speed: 250m / min

[0264] Cutting depth: 1.5mm

[0265] Feed rate: 0.4mm / rev.

[0266] Cutting times: 20 times

[0267] The results of the cutting test are shown in Table 10. In Comparative Examples 11 to 15, the life was reached before the number of cutting passes reached 20 due to chipping or flank wear (life judgment criterion: flank wear width 0.4 mm), so the number of cutting passes to reach the life is shown.

[0268] [Table 10]

[0269]

[0270] From the results shown in Table 10, it can be seen that Examples 11 to 15 have less wear, no chipping occurs, and both hardness and toughness are improved, thereby exhibiting excellent cutting performance for a long time.

[0271] In contrast, in Comparative Examples 11 to 15, the wear amount was large or chipping occurred, and the service life was reached in a short time.

[0272] The embodiments disclosed above are merely illustrative in all aspects and are not restrictive. The scope of the present invention is expressed by the claims rather than the embodiments described above, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0273] Description of Reference Numerals

[0274] 1Ti atom

[0275] 2 Anionic sites (N atoms)

[0276] 3 Anionic sites (C atoms)

[0277] 4 Cation sites (any atom among Ti, V, Zr and Nb or any atom among Ti, V, Zr, Nb, Hf and Ta (Hf and Ta are selected according to the composition))

Claims

1. A surface-coated cutting tool comprising a substrate and a coating layer on the surface of the substrate, characterized in that: The coating layer comprises a composite carbonitride layer, The average thickness of the composite carbonitride layer is 1.0 μm or more and 20.0 μm or less, When the total atomic ratio of the metal components in the composite carbonitride layer is 1, the metal components Ti, V, Zr, and Nb are contained at atomic ratios a1, a2, a3, and a4 of the metal components, respectively. When the total atomic ratio of the non-metallic components in the composite carbonitride layer is 1, the non-metallic components C and N are contained at atomic ratios b1 and b2 of the non-metallic components, respectively. The composite carbonitride layer further contains inevitable impurities, The a1, a2, a3, a4, b1, and b2 are as follows: 0.01≤a1≤0.60 0.01≤a2≤0.60 0.01≤a3≤0.60 0.01≤a4≤0.60 0.20≤b1≤0.80 0.20≤b2≤0.80, When n=4 and m=2, S represented by Formula 1 config is greater than 0.80R, where ln in formula 1 is the natural logarithm, R is the gas constant, The composite carbonitride layer comprises grains having a NaCl-type face-centered cubic structure, 2. The surface-coated cutting tool according to claim 1, characterized in that: The composite carbonitride layer further contains at least one of Hf and Ta as the metal component, and the atomic ratios of Hf and Ta are a5 and a6, respectively. The a5 and a6 are as follows: a5<0.01 a6<0.01, When n=6 and m=2, S represented by Formula 1 config is 0.80R or more, wherein when i = 5 or 6 a i When it is zero, it does not contain i ln(a i )=0.

3. The surface-coated cutting tool according to claim 1 or 2, characterized in that: The composite carbonitride layer includes 0.50 atomic % or less of Cl.

Citation Information

Patent Citations

  • CVD-coated article and CVD process of making the same

    US20160298233A1

  • Superhard strong toughness and high-entropy alloy nitride nano-composite coating carbide blade and preparation method thereof

    CN108642449A

  • Coated cutting tool

    CN112439935A

  • PVD coatings comprising multi-anion high entropy alloy oxy-nitrides

    CN113966408A

  • Coated cutting tool member

    CN1675015A