Atomizing core and atomizing device
The atomizer core with a tantalum film addresses dry-burning and wet-burning failures by enhancing resistance and corrosion resistance, ensuring a longer service life.
Patent Information
- Application Number
- CN202310640516.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
Existing atomizer cores suffer from both dry-burning and wet-burning failures due to high-temperature electrochemical corrosion, leading to a short service life.
An atomizer core with a tantalum film on the heating film, having a melting point above 1400°C and resistivity less than 5*10^-7 Ωm, providing resistance more than five times that of the heating film, enhances both dry-burning and wet-burning resistance.
The atomizer core exhibits improved high-temperature oxidation resistance and extended life by preventing electrochemical corrosion, maintaining resistance within acceptable limits under both dry and wet burning conditions.
Smart Images

Figure CN119054958A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an atomization core and an atomization device, belonging to the technical field of electronic cigarettes. Background Art
[0002] In new electronic atomization components, thin-film heating films are mostly used to replace traditional thick films. The advantages of thin-film heating films are good material consistency, thin film thickness, and they will not fill the micropores on the heating surface of the porous substrate, which will not affect the transmission speed of the smoke oil and can achieve higher atomization efficiency. However, if there is insufficient liquid supply during the heating and atomization process, the heating film will dry burn, and the temperature can even reach over 1000°C, which can easily lead to the failure of the heating film due to dry burning; on the other hand, atomization is achieved by heating the heating film with electricity (the potential difference is usually around 3-4V). At the same time, due to the wide variety of atomization media, the components of which contain some corrosive substances, and the working temperature of the heating film is as high as 300°C. Therefore, during the atomization process, the metal heating film is very prone to high-temperature electrochemical corrosion, which leads to corrosion failure of the heating film.
[0003] Although some existing heating film materials can meet certain dry-burning performance requirements, as the atomization temperature increases and the requirements for wet-burning life increase, these heating films are very susceptible to corrosion under high-temperature electrochemical corrosion conditions, resulting in excessive resistance changes after long-term operation. Therefore, there is an urgent need to develop a long-life atomization core structure that is resistant to both dry-burning and wet-burning. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an atomizer core to solve the problem that the existing atomizer core does not have both dry burning resistance and wet burning resistance and has a short service life. The present invention adopts the following technical solutions:
[0005] An atomizer core comprises a substrate, wherein a tantalum film is provided on a surface of a heating film away from the substrate; wherein the heating film has a melting point of more than 1400°C and a resistivity of less than 5*10 -7 The tantalum film is made of a metal single substance or alloy material with a resistance of Ωm; the resistance of the tantalum film is more than 5 times that of the heating film.
[0006] Optionally, the tantalum film completely covers the surface of the heating film away from the substrate.
[0007] Optionally, the resistance of the tantalum film is 5 to 10 times the resistance of the heating film.
[0008] Optionally, the alloy has a melting point of more than 1400°C and a resistivity of less than 5*10 -7 Ωm metal alloy.
[0009] Optionally, the heating film has a melting point of 1400-4000°C and a resistivity of 1*10 -8Ωm~5*10 -7 Ωm metal single substance or alloy material.
[0010] Optionally, the thickness of the tantalum film is 50-500 nm.
[0011] Optionally, the thickness of the tantalum film is 300-400 nm.
[0012] Optionally, the tantalum film is of β-Ta crystal type.
[0013] Optionally, the tantalum film is made by a physical vapor deposition method.
[0014] Optionally, the heating film has a thickness of 300-5000nm.
[0015] Optionally, the heating film is made of at least one of Ti single substance, Cr single substance, Mo single substance, Nb single substance, Ti alloy, Cr alloy, Mo alloy, Nb alloy, and iron-based alloy materials.
[0016] Optionally, the heating film is made of stainless steel.
[0017] Optionally, the heating film is a stainless steel heating film, and the thickness of the heating film is more than 3 times the thickness of the tantalum film.
[0018] Optionally, the heating film is a stainless steel heating film, and the thickness of the heating film is 3 to 20 times the thickness of the tantalum film.
[0019] Optionally, the heating film includes the following components by mass fraction:
[0020] Fe 67~72%, Cr 16~18%, Ni 10~12%, Mo 2~3%.
[0021] Optionally, the heating film comprises the following components by mass fraction: Fe 67-72%, Cr 16-18%, Ni 10-12%, Mo 2-3%, and the mass fraction of other elements is less than 1%.
[0022] Optionally, the heating film is made by physical vapor deposition.
[0023] Optionally, a protective layer is provided on the surface of the tantalum film away from the heating film.
[0024] Optionally, the atomizer core further includes two pins, which are respectively arranged on two opposite sides of the heating film and are electrically connected to the heating film.
[0025] Optionally, a protective layer is provided on the pin.
[0026] Optionally, the protective layer is made of at least one of aluminum oxide, silicon oxide, aluminum oxynitride, and silicon oxynitride.
[0027] Optionally, the protective layer is made by physical vapor deposition or chemical vapor deposition.
[0028] The present invention also provides an atomization device, which includes at least one of the above-mentioned atomization cores.
[0029] Compared with the prior art, the present invention has the following technical effects:
[0030] The atomizer core of the present invention is provided with a heating film on a substrate, and a tantalum film is provided on a surface of the heating film away from the substrate; wherein the heating film has a melting point of more than 1400°C and a resistivity of less than 5*10 -7 The resistance of tantalum film is more than 5 times that of heating film. Tantalum is one of the most chemically stable metals, and it is easy to form a passivation film on the surface with very high electrochemical corrosion resistance, especially for the medium environment with chloride ions, which can effectively isolate the electronic cigarette atomization medium and the heating film. At the same time, the heating film material adopts a melting point of more than 1400℃ and a resistivity of less than 5*10 -7 Ωm metal single substance or alloy material, and control the resistance of the tantalum film to be more than 5 times the resistance of the heating film, so as to ensure that the current mainly passes through the low-resistance heating film layer, the tantalum film does not generate high heat, and the heat is mainly concentrated at the heating film end. This setting can not only effectively improve the high-temperature oxidation resistance of the heating film and the tantalum film, so that the atomizer core as a whole has a strong dry-burning resistance, but also the tantalum film can significantly avoid the high-temperature electrochemical corrosion of the atomizing medium on the heating film, improve the high-temperature wet-burning resistance, and extend the life. Therefore, the atomizer core of the present invention has both strong dry-burning resistance and strong wet-burning resistance, and is a long-life atomizer core. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the atomizer core structure of Example 1;
[0032] Markings in the figure are 1. substrate, 2. heating film, 3. tantalum film, 4. pin, and 5. protective layer.
[0033] Figure 2 It is the wet burning resistance change rate of the heating element in Example 1 (wet burning 1200 puffs).
[0034] Figure 3 It is the wet burning resistance change rate of the heating element in comparative example 1 (1000 puffs of wet burning). DETAILED DESCRIPTION
[0035] The present invention proposes an atomizer core, comprising a substrate, a heating film is arranged on the substrate; a tantalum film is arranged on the surface of the heating film away from the substrate; the melting point of the heating film is above 1400°C; the resistivity of the heating film is lower than 5*10 -7 The tantalum film is made of a material with a resistance of more than 5 times that of the heating film. Tantalum is one of the most chemically stable metals. It is easy to form a passivation film on the surface with very high electrochemical corrosion resistance, especially for a medium environment with chloride ions. The tantalum film in this atomizer core can effectively protect the heating film, and significantly improve the wet burning resistance and life of the atomizer core. This atomizer core meets the following two conditions at the same time: the heating film material has a high melting point and low resistivity; the resistance of the tantalum film is more than 5 times the resistance of the heating film. This allows the current to pass mainly through the low-resistance heating film layer, and the tantalum film has a low heat generation, and its high-temperature oxidation resistance is improved, which can ensure that the dry burning performance standard is met. At the same time, the tantalum film can significantly avoid the high-temperature electrochemical corrosion of the atomization medium on the heating film, improve the high-temperature wet burning resistance, and extend the life. Therefore, the atomizer core of the present invention has both strong dry burning resistance and strong wet burning resistance, and is a long-life atomizer core.
[0036] In an optional embodiment, the tantalum film completely covers the surface of the heating film away from the substrate. The ratio of the resistance of the tantalum film to the resistance of the heating film can be achieved by adjusting the thickness of the tantalum film. In an optional embodiment, the thickness of the tantalum film is 50-500nm. For example, the thickness of the tantalum film can be selected to be 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm. The thickness of the tantalum film is preferably 300-400nm. The thickness of the tantalum film is relatively low, and the stress of the film layer itself is reduced. During the long-life operation, the cracking failure of the dielectric protective layer due to fatigue thermal stress can be avoided.
[0037] In an optional embodiment, the tantalum film is a β-Ta crystal. The β-Ta crystal tantalum film has a high resistivity (resistivity 2*10 -6 Ω.m), less heat is generated at the same thickness.
[0038] In an optional embodiment, the thickness of the heating film is 1400-5000nm. For example, the thickness of the tantalum film can be selected to be 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm, 2500nm, 3000nm, 3500nm, 4000nm, 4500nm, 5000nm. This kind of heating film is a thin film heating film below 5000nm. In an optional embodiment, the tantalum film is made by a physical vapor deposition method.
[0039] In an optional embodiment, the heating film can be made of Ti, Cr, Mo, Nb, alloys and other materials with high melting points (above 1400 degrees Celsius) and low resistivity (less than 5*10 -7 Ωm) material. In an optional embodiment, the heating film is made of stainless steel. In an optional embodiment, the stainless steel heating film includes, by mass fraction, 67-72% Fe, 16-18% Cr, 10-12% Ni, and 2-3% Mo. In an optional embodiment, the heating film material is a stainless steel heating film, and the thickness of the heating film is more than 3 times the thickness of the tantalum film to ensure that the resistance of the tantalum film is greater than 5 times the resistance of the heating film. In an optional embodiment, the heating film is made of materials such as Ti, Cr, Mo, and Nb. This is because the current stainless steel heating film, due to the limitations of resistivity and film thickness, has a maximum aspect ratio of 3:1, which has certain limitations on the design of heating patterns. In order to improve the aspect ratio range of the heating film, a high melting point and low resistivity single metal can be used as the heating film, and the Ta layer can also be covered to ensure its dry and wet burning performance. In an optional embodiment, the heating film is made by physical vapor deposition.
[0040] In an optional embodiment, a protective layer is provided on the surface of the tantalum film away from the heating film. In an optional embodiment, the protective layer is made of at least one of insulating materials such as aluminum oxide, silicon oxide, aluminum oxynitride, silicon oxynitride, etc. In an optional embodiment, the protective layer is made by physical vapor deposition or chemical vapor deposition. In an optional embodiment, the atomization core also includes two pins, which are respectively arranged on opposite sides of the heating film and are electrically connected to the heating film. The function of the pin is to energize the heating film. In an optional embodiment, a protective layer is also provided on the pin. The protective layer reduces the corrosion of the electronic cigarette medium to the tantalum film, the heating film and the pin.
[0041] The present invention also proposes an atomizing device, which includes at least one of the above-mentioned atomizing cores. The above-mentioned atomizing core can achieve the following performance: Heating film dry burning performance> 7.5W (for 3.5mm 2 Heating film area, porosity 20%, 7.5W constant power on for 3s and off for 8s, dry burning in air for 10 cycles, heating film resistance change <20%). Heating film wet burning performance>1200 puffs (tested with strawberry watermelon ice e-liquid, 7.5W for 3s and off for 15s, 1200 puffs resistance change is not higher than 21%).
[0042] The following examples are provided only for the purpose of illustrating the present invention in more detail. The materials involved in the examples are all commercially available products. The following examples are provided for a better understanding of the present invention, are not limited to the best mode of implementation, and do not limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the enlightenment of the present invention or by combining the features of the present invention with other prior arts falls within the protection scope of the present invention.
[0043] The calculation method of the resistance ratio of the tantalum film to the heating film in each embodiment is as follows: the resistance of the single-layer heating film pattern tested is R1, and the comprehensive resistance of the heating film covered with the tantalum film tested is R, and the tantalum film resistance R2 is calculated by the following formula:
[0044] R2 = R*R1 / (R1-R);
[0045] The resistance ratio of the tantalum film to the heating film is calculated as R2 / R1.
[0046] The test method for resistance change in each embodiment and comparative example is as follows: dry-burning test resistance change method: first test the initial resistance R0 of the heating film, the heating film is energized at a constant power of 7.5W for 3s and then stopped for 8s, and dry-burned in the air for 10 cycles. The resistance R10 of the heating film after 10 cycles of dry-burning can be calculated, and the resistance change rate ΔR before and after dry-burning can be calculated as (R10-R0) / R0.
[0047] Wet burning test resistance change method: load the heating element with e-liquid, test the initial resistance R0 after loading, select a 7.5w constant power battery, power on for 3s and then stop for 15s, test the resistance Rx of the heating film of the cartridge after 150 puffs, and calculate the resistance change rate ΔR=(Rx-R0) / R0 before and after wet burning.
[0048] The physical vapor deposition method described in each embodiment is: using magnetron sputtering equipment, preparing the metal conductive layer by a direct current (DC) sputtering method, and preparing the insulating protective film by a radio frequency (RF) method.
[0049] The strawberry-watermelon ice fruit-flavored e-liquid in each embodiment is: strawberry-watermelon flavored e-liquid (40 mg) produced by Shenzhen Yupeng Technology Co., Ltd.
[0050] Example 1
[0051] like Figure 1As shown, this embodiment proposes an atomization core, including a heating substrate 1, which is an array pore structure with a porosity of 20%. A heating film 2 of 316 stainless steel is formed on the heating substrate by physical vapor deposition, and the heating film 2 contains by mass fraction: Fe~70%, Cr~16.5%, Ni~10.5%, Mo~2.5%, and the rest are inevitable elements such as C and S in stainless steel. The thickness of the heating film 2 is 1300nm, and a tantalum film 3 is formed on the side of the heating film 2 away from the substrate 1 by physical vapor deposition. The thickness of the tantalum film is 300nm.
[0052] A 50nm thick 316 stainless steel layer and a 2um thick Ag layer are deposited on the pins 4 on both sides of the heating film by physical vapor deposition, so that the pins 4 are connected to the heating film.
[0053] A 100 nm thick Al2O3 protective film 5 is deposited on the pin and on the surface of the tantalum film.
[0054] Use the atomizer core to assemble an electronic cigarette atomizer and further process it into an electronic cigarette. Perform dry burning and wet burning tests:
[0055] Dry burning and wet burning tests were conducted. Dry burning capacity: 7.5W dry burning 10 puffs resistance change <20% (7.5W constant power on 3s and stop 8s dry burning in air); wet burning capacity: Strawberry Watermelon Ice Fruity E-liquid 7.5W puff 1200 puffs resistance change 21% (7.5W puff 3s and stop 15s, capacity 55mL). Figure 2 As shown, the resistance increase of the heating element was relatively high before 600 puffs (which was mainly due to a certain amount of electrochemical corrosion of the pin Ag). After 600 puffs, the resistance increase tended to be gentle, indicating that the high-temperature electrochemical corrosion of the heating film tended to stagnate.
[0056] Comparative Example 1
[0057] The atomizer core in this comparative example does not have a tantalum film on the heating film, and the rest is the same as in Example 1, using the same 316 stainless steel heating film. The electronic cigarette atomizer is assembled using the heating film structure, and further processed into an electronic cigarette. Dry burning and wet burning tests are carried out:
[0058] Dry burning and wet burning tests were conducted. Dry burning capacity: 7.5W dry burning 10 puffs resistance change <20% (7.5W constant power on 3s and stop 8s dry burning in air); wet burning capacity: 7.5W strawberry watermelon ice fruit flavor e-liquid 750 puffs resistance change <20%, and the resistance change from 750 to 1000 puffs increased to 46% (7.5W puff 3s stop 15s, capacity 55mL). Figure 3 As shown, the resistance of the heating element increased significantly after 800 puffs, indicating that the heating film was severely electrochemically corroded, resulting in a sharp increase in resistance.
[0059] In Examples 2 to 6 and Comparative Examples 2 to 7, the substrate, pore size, porosity, and dry and wet burning test conditions are the same as those in Example 1, except that the heating film material, tantalum film thickness, and protective layer thickness are changed. The relevant dry and wet burning test results are shown in Table 1.
[0060] Table 1, dry burning and wet burning test results
[0061]
[0062]
[0063] From the above experimental results, it can be seen that the provision of a tantalum film can significantly improve the high temperature wet burning resistance of the atomizer core. From the results of Example 1 and Comparative Example 2, it can be seen that when the thickness of the tantalum film is too large, the atomizer core will have insufficient dry burning resistance. From the results of Comparative Example 7, it can be seen that when low melting point Al is used as the heating film, the atomizer core has very poor dry burning resistance.
[0064] In summary, the present invention has high melting point (above 1400°C), low resistivity (less than 5*10 -7 A tantalum film is arranged on a heating film with a resistance of more than 5 times that of the heating film, so that an atomizer core with strong resistance to dry burning and strong resistance to wet burning can be obtained. The atomizer core has a long service life, the dry burning performance of the heating film is greater than 7.5W, and the resistance change after 1200 puffs at 7.5W is not higher than 21%.
[0065] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. An atomizer core, comprising a substrate, characterized in that: The substrate is provided with a heating film, and a tantalum film is provided on the surface of the heating film away from the substrate; wherein the heating film has a melting point of more than 1400°C and a resistivity of less than 5*10 -7 Made of metal single substance or alloy material of Ωm; The resistance of the tantalum film is more than 5 times that of the heating film.
2. The atomizer core according to claim 1, characterized in that: The thickness of the tantalum film is 50-500nm; Preferably, the thickness of the tantalum film is 300-400 nm.
3. The atomizer core according to claim 1, characterized in that: The tantalum film is of β-Ta crystal type.
4. The atomizer core according to claim 1, characterized in that: The tantalum film is produced by a physical vapor deposition method.
5. The atomizer core according to claim 1, characterized in that: The heating film has a thickness of 300-5000nm.
6. The atomizer core according to claim 1, characterized in that: The heating film is made of at least one of Ti single substance, Cr single substance, Mo single substance, Nb single substance, Ti alloy, Cr alloy, Mo alloy, Nb alloy, and iron-based alloy materials.
7. The atomizer core according to claim 1, characterized in that: The heating film is made of stainless steel; Preferably, the heating film is a stainless steel heating film, and the thickness of the heating film is more than 3 times the thickness of the tantalum film; Further preferably, the heating film comprises the following components by mass fraction: Fe 67~72%, Cr 16~18%, Ni 10~12%, Mo 2~3%.
8. The atomizer core according to claim 1, characterized in that: The heating film is made by a physical vapor deposition method.
9. The atomizer core according to claim 1, characterized in that: A protective layer is provided on the surface of the tantalum film away from the heating film.
10. The atomizer core according to claim 9, characterized in that: The protective layer is made of at least one of aluminum oxide, silicon oxide, aluminum oxynitride and silicon oxynitride.
11. The atomizer core according to claim 9, characterized in that: The protective layer is made by physical vapor deposition or chemical vapor deposition.
12. An atomizing device, characterized in that: The atomizing device comprises the atomizing core according to any one of claims 1 to 11.
Citation Information
Cited By
Atomization core and atomization apparatus
EP4721596A1