Aluminum silicate filter membrane based composite material as well as preparation method and application thereof
By using catalysts such as elemental silver, manganese oxide, and tricobalt oxide on the aluminum silicate filter membrane, the problems of low formaldehyde removal efficiency and limited loading of catalysts in the prior art are solved, and efficient formaldehyde catalytic decomposition and adsorption are achieved. Secondary contamination is avoided and the preparation process is simplified.
Patent Information
- Application Number
- CN202310624086.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, powder-type catalysts have low efficiency in catalyzing formaldehyde degradation at room temperature, limited load on the support and easy to fall off, and the traditional slow adsorption rate leads to secondary contamination.
Aluminum silicate filter membrane is used as the matrix, and catalysts such as elemental silver, manganese oxide, tricobalt tetroxide are used to immerse and heat treatment through a mixed solution of manganese salt, silver salt, cobalt salt and reducing agent to firmly adhere to the surface and interior of the aluminum silicate filter membrane. , form an efficient catalyst support to achieve catalytic decomposition and adsorption of formaldehyde.
It realizes uniform loading of the catalyst, firmly adheres to it and is not easy to fall off, improves the catalytic decomposition efficiency of formaldehyde, avoids secondary pollution, and simplifies the preparation process, which is suitable for industrial applications.
Smart Images

Figure CN119056439A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of air purification, and specifically relates to an aluminum silicate filter membrane-based composite material and a preparation method and application thereof. Background Art
[0002] In recent years, with the continuous improvement of the quality of life, people have gradually realized the importance of indoor air quality. Formaldehyde is a highly toxic volatile organic compound. It is colorless but irritating. It has the characteristics of a long incubation period and persistent pollution. If it is exposed to an environment with excessive formaldehyde content for a long time, it will erode people's respiratory system, circulatory system and nervous system. Due to its serious carcinogenicity, blood toxicity and genetic toxicity, it will bring serious physiological diseases to people, and even cause lung cancer, leukemia, brain cancer and other diseases. In order to reduce the huge trauma caused by formaldehyde pollution to the human body, people mostly use plant absorption and physical adsorption purification to remove indoor formaldehyde. Among them, plant absorption is mainly carried out by green plants such as green radish and aloe vera for absorption and purification; physical adsorption is mainly activated carbon, diatomaceous earth, bentonite, etc. This type of adsorption material cannot achieve the decomposition of formaldehyde. After adsorption saturation, it cannot, which will form secondary pollution. Another way is to use catalytic oxidation technology to oxidize formaldehyde into carbon dioxide and water to reduce the content. The catalytic oxidation method can improve the efficiency of formaldehyde degradation and solve the problem of secondary pollution by relying on the oxidizability and surface properties of metal oxides. At present, there have been breakthroughs and progress in the use of catalytic oxidation to degrade formaldehyde at room temperature.
[0003] Chinese invention patent CN108262031A discloses a glass fiber non-woven fabric-supported photocatalyst, which supports regular morphology of TiO2 photocatalyst spherical powder on glass fiber non-woven fabric, and turns on ultraviolet light to achieve formaldehyde degradation and catalyst recovery. This method uses an immersion method to support the catalyst on the glass fiber non-woven fabric. Due to the structural properties of the glass fiber non-woven fabric itself, it cannot be folded in any direction, and the loading capacity is limited.
[0004] Chinese invention patent CN114433244A discloses a filter membrane and preparation method for catalytic degradation of formaldehyde, in which catalyst particles are attached to a fiber layer, and at least part of the catalyst particles are located inside a mesh structure, and the catalyst loaded inside the matrix catalytically degrades formaldehyde, thereby achieving the effect of air purification. This method uses spraying, gluing or dipping to load particles on the matrix, which cannot form a uniform and stable catalyst coating, and the loading amount is also limited, resulting in the phenomenon of powder catalyst falling from the matrix, and the entire preparation process is cumbersome.
[0005] In summary, the powder catalysts in the prior art have low efficiency in catalytic degradation of formaldehyde at room temperature, and the loading amount on the carrier is limited and easy to fall off, and the traditional adsorption rate is slow and easy to cause secondary pollution. Summary of the invention
[0006] The present invention aims to provide an aluminum silicate filter membrane-based composite material for catalytic degradation of formaldehyde at room temperature, so as to solve the problems in the prior art that the powder-type catalyst has low efficiency in catalytic degradation of formaldehyde at room temperature, the loading amount on the carrier is limited and easy to fall off, and the traditional adsorption rate is slow, resulting in secondary pollution.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] The present invention provides an aluminum silicate filter membrane-based composite material, comprising a matrix and a catalyst, wherein the matrix comprises an aluminum silicate filter membrane with adsorptivity, ductility and air permeability, and the catalyst comprises any one of elemental silver, manganese oxide and cobalt tetroxide or a mixture of two or more thereof; the catalyst is firmly adhered to the surface and interior of the aluminum silicate filter membrane.
[0009] Furthermore, the aluminum silicate filter membrane has a thickness of 2 mm to 10 mm and a pore size of 1 μm to 50 μm.
[0010] Furthermore, the content of the catalyst in the aluminum silicate filter membrane-based composite material is 2.7-88%.
[0011] Furthermore, the catalyst loading is 0.0001-0.02 g / cm 3 .
[0012] The present invention also provides a method for preparing the aluminum silicate filter membrane-based composite material, comprising:
[0013] Provide any one of manganese salt, silver salt and cobalt salt or a combination of two or more thereof and mix with a reducing agent to form a mixed solution, immerse an aluminum silicate filter membrane in the mixed solution, discharge the remaining liquid and perform heat treatment to obtain an aluminum silicate filter membrane-based composite material.
[0014] Furthermore, before the aluminum silicate filter membrane is immersed in the mixed solution, the aluminum silicate filter membrane is pretreated. Specifically, the pretreatment includes treating the aluminum silicate filter membrane at 80-550° C. for 0.5-4 h.
[0015] Furthermore, the heat treatment includes heat treating the aluminum silicate filter membrane at 200 to 500° C. for 1 to 10 hours in an air atmosphere.
[0016] Furthermore, the manganese salt includes any one of manganese nitrate, manganese sulfate, and manganese chloride, or a combination of two or more thereof.
[0017] Furthermore, the silver salt includes any one of silver nitrate and silver fluoride or a combination of the two.
[0018] Furthermore, the cobalt salt comprises cobalt nitrate.
[0019] Furthermore, the reducing agent includes any one of glycine, citric acid, and urea, or a combination of two or more thereof.
[0020] Furthermore, the mass ratio of the reducing agent to any one of the manganese salt, the silver salt, and the cobalt salt or a combination of two or more thereof is 1:4-12.
[0021] Furthermore, the immersion time is 0.5-24h.
[0022] Furthermore, before the heat treatment, the aluminum silicate filter membrane is dried at 80-100° C. for 10-24 hours.
[0023] Furthermore, the concentration of manganese ions in the manganese salt is 0.06mol / L-3.5mol / L; the concentration of silver ions in the silver salt is 0.3mol / L-2mol / L; and the concentration of cobalt ions in the cobalt salt is 0.1mol / L-2mol / L.
[0024] The invention discloses an application of the aluminum silicate filter membrane-based composite material in air purification and pollutant degradation.
[0025] The method of using the aluminum silicate filter membrane-based composite material to purify air includes contacting the aluminum silicate filter membrane-based composite material provided by the present invention with a volatile gas, in particular, contacting with a gas containing formaldehyde, and the formaldehyde concentration is 3 to 10 ppm.
[0026] Compared with the prior art, the beneficial effects of the present invention are at least:
[0027] (1) The preparation method of the aluminum silicate filter membrane-based composite material provided by the present invention can firmly attach the catalyst to the aluminum silicate filter membrane, making it difficult to fall off, with uniform loading, and the preparation method is simple.
[0028] (2) The aluminum silicate filter membrane-based composite material provided by the present invention can not only catalyze the decomposition of formaldehyde, but also adsorb formaldehyde, achieving formaldehyde adsorption and conversion at the same time, further improving the efficiency of formaldehyde degradation and avoiding secondary pollution.
[0029] (3) The aluminum silicate filter membrane-based composite material prepared by the present invention can be used as a flexible catalytic filter screen built into commercial central air conditioners, air purifiers and other cabinets, and can be combined with other purification units to improve air purification efficiency, which is easy to promote industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is the X-ray diffraction pattern of the manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 of the present invention.
[0032] Figure 2 This is the X-ray diffraction pattern of the silver / cobalt oxide / aluminum silicate filter membrane composite material prepared in Example 13 of the present invention.
[0033] Figure 3 This is a scanning electron microscope image of the manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0034] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be clearly and completely described below. It is mainly an aluminum silicate filter membrane-based composite material and its preparation method and application.
[0035] The invention provides an aluminum silicate filter membrane-based composite material, comprising a matrix and a catalyst.
[0036] The aluminum silicate filter membrane-based composite material includes an aluminum silicate filter membrane as a matrix and a catalyst as an active component. The catalyst is attached to the surface and interior of the aluminum silicate filter membrane, and at least part of the catalyst particles are located inside the carrier.
[0037] As a carrier, the aluminum silicate filter membrane itself has adsorption properties. In addition, the aluminum silicate filter membrane is cheap, easy to obtain, and has high temperature and oxidation resistance, which can improve the stability of the catalyst.
[0038] Furthermore, the preparation method of the aluminum silicate filter membrane-based composite material includes:
[0039] Provide any one of manganese salt, silver salt and cobalt salt or a combination of two or more thereof and mix with a reducing agent to form a mixed solution, immerse an aluminum silicate filter membrane in the mixed solution, drain the remaining liquid, and perform heat treatment to obtain an aluminum silicate filter membrane-based composite material.
[0040] The present application also provides an air purification method, comprising: introducing polluted organic gas into the aluminum silicate filter membrane-based composite material, and bringing the aluminum silicate filter membrane-based composite material into contact with the polluted organic gas, thereby at least partially degrading the polluted organic gas. Using a detector to detect changes in the concentration of the polluted organic gas.
[0041] In some specific embodiments, the polluted organic gas is formaldehyde, and the aluminum silicate filter membrane-based composite material degrades formaldehyde at room temperature.
[0042] Furthermore, the concentration of the formaldehyde gas is 3-10 ppm.
[0043] In some specific embodiments, the purification method specifically includes: placing the aluminum silicate filter membrane-based composite material in a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL and filled with quartz wool, so that it is in contact with air carrying formaldehyde, thereby catalytically degrading at least part of the formaldehyde.
[0044] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention, and do not have any limiting effect on them. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.
[0045] Example 1
[0046] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 83.7g of 50wt% in H2O manganese nitrate aqueous solution was weighed and added with 25mL deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 3.5mol / L, and then 6.92g of glycine was weighed and dissolved in the manganese nitrate aqueous solution to form a mixed solution with a concentration of 4.8mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing, dried at 80℃ for 10h, and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method.
[0047] In this embodiment, the chemical reaction between nitrate and glycine is usually an exothermic reaction, which can maintain the heat required for the reaction. The sample was placed in a box-type resistance furnace and kept warm at 400°C for 1 hour. During this period, a catalyst coating was formed on the surface and inside of the aluminum silicate filter membrane through combustion. The resulting composite material is complete and can be twisted at will without breaking or falling off. The manganese oxide layer has a loading content of 88%, and the manganese oxide loading (weight of catalyst / volume of aluminum silicate filter membrane) is 0.02g / cm3 .
[0048] Example 2
[0049] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 83.7g of 50wt% in H2O manganese nitrate aqueous solution was weighed and added with 124mL deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 1.4mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate aqueous solution to form a mixed solution with a concentration of 1.9mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material was complete and could be twisted at will without breaking or falling off. The manganese oxide layer loading content is 36%, and the catalyst loading is 0.0063 g / cm 3 .
[0050] Example 3
[0051] Cut the aluminum silicate filter membrane with a thickness of 5 mm (pore size 1 μm-50 μm) into a circular filter disc with a diameter of 5 cm, lay it flat on tin foil, put it into a box-type resistance furnace, and heat treat it at 550°C for 4 hours in an air atmosphere. The pretreated aluminum silicate filter membrane is sealed with tin foil and placed in a desiccator for storage. Weigh 83.7g of 50%wt%in H2O manganese nitrate aqueous solution and add 248mL of deionized water to dilute it to a manganese ion concentration of 0.8mol / L in the manganese nitrate aqueous solution, and then weigh 6.92g of glycine and dissolve it in the manganese nitrate solution to form a mixed solution with a concentration of 1.1mol / L. Immerse the dried aluminum silicate filter membrane in the above mixed solution for 4 hours, drain the excess liquid by squeezing, dry it at 80°C for 10 hours, and place it in a box-type resistance furnace at 400°C for 1 hour to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material is complete and can be twisted at will without any breakage or slag. The manganese oxide layer loading content is 21% and the catalyst loading is 0.0038g / cm 3 .
[0052] Example 4
[0053] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 372mL of deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.5mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate aqueous solution to form a mixed solution with a concentration of 0.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material was complete and could be twisted at will without breaking or falling off. The manganese oxide layer loading is 15% and the catalyst loading is 0.0025 g / cm 3 .
[0054] See also Figure 1 , is an X-ray diffraction pattern of the manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 of the present invention, which shows that the prepared manganese oxide / aluminum silicate filter membrane composite material contains a manganese oxide phase.
[0055] See also Figure 3 , is a scanning electron microscope image of the manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 of the present invention. It can be seen intuitively that manganese oxide adheres to the surface of the aluminum silicate filter membrane substrate and the inside of the aluminum silicate filter membrane substrate.
[0056] Example 5
[0057] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added to 496mL of deionized water to dilute to a manganese ion concentration of 0.4mol / L, and then 6.92g of glycine was weighed and dissolved in the manganese nitrate solution to form a mixed solution with a concentration of 0.6mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing, dried at 80℃ for 10h, and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of manganese oxide composite layer is 8%, and the loading of catalyst is 0.0013 g / cm 3 . .
[0058] Example 6
[0059] A 2mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 372mL of deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.5mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate aqueous solution to form a mixed solution with a concentration of 0.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material was complete and could be twisted at will without breaking or falling off. The loading of manganese oxide composite layer is 7%, and the loading of catalyst is 0.0010g / cm 3 .
[0060] Example 7
[0061] A 10mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 372mL of deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.5mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate solution to form a mixed solution with a concentration of 0.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material was complete and could be twisted at will without breaking or falling off. The manganese oxide composite layer loading is 25%, and the catalyst loading is 0.0022 g / cm 3 .
[0062] Example 8
[0063] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 372mL of deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.5mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate solution to form a mixed solution with a concentration of 0.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by suction filtration. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material is complete and can be twisted at will without any breakage or slag. The manganese oxide layer loading is 11% and the catalyst loading is 0.0020 g / cm 3 .
[0064] Example 9
[0065] A 2mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 2232mL of deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.06mol / L. Then 6.92g of glycine was weighed and dissolved in the manganese nitrate solution to form a mixed solution with a concentration of 0.1mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h. After filtering off the excess liquid, it was placed in an 80℃ oven for drying for 10h, and then placed in a 200℃ box-type resistance furnace for insulation for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by an in-situ combustion method. The obtained composite material is complete and can be twisted at will without any breakage or slag. The loading of manganese oxide composite layer is 2.7% and the loading of catalyst is 0.0001g / cm 3 .
[0066] Example 10
[0067] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. 83.7g of 50%wt%in H2O manganese nitrate aqueous solution was weighed and added with 372mL deionized water to dilute the manganese ion concentration of the manganese nitrate aqueous solution to 0.5mol / L, and then 6.92g of glycine was dissolved in the manganese nitrate solution to form a mixed solution with a concentration of 0.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. The box-type resistance furnace was heated to 400℃ and kept warm for 1h to obtain a manganese oxide / aluminum silicate filter membrane composite material prepared by the solution combustion method. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of manganese oxide composite layer is 13.8%, and the loading of catalyst is 0.0021 g / cm 3 .
[0068] Embodiment 11
[0069] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 1.4551g Co(NO3)2·6H2O was weighed and dissolved in water to form a solution with a cobalt ion concentration of 0.1mol / L. Then 1.0426g glycine was weighed and dissolved in 50mL deionized water and mixed with the Co(NO3)2·6H2O solution to form a mixed solution with a concentration of 0.2mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a cobalt oxide / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of the cobalt oxide / aluminum silicate filter membrane composite material is 15%, and the catalyst loading is 0.0021 g / cm 3 .
[0070] Example 12
[0071] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5.5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 550℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. Weigh 2.5480g Ag NO3 and dissolve it in water to form a solution with a silver ion concentration of 0.3mol / L. Then weigh 1.0426g glycine and mix it with the Ag NO3 solution and add 45mL deionized water to form a mixed solution with a concentration of 0.6mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing. It was dried at 80℃ for 10h and placed in a box-type resistance furnace at 400℃ for 1h to obtain a silver / aluminum silicate filter membrane composite material prepared by in-situ combustion method. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of silver / aluminum silicate filter membrane composite material is 9%, and the loading of catalyst is 0.0015 g / cm 3 .
[0072] Embodiment 13
[0073] Cut a 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) into a circular filter disc with a diameter of 5cm, lay it flat on tin foil, put it into a box-type resistance furnace, and heat treat it at 550℃ for 4h in air atmosphere. The pretreated aluminum silicate filter membrane is sealed with tin foil and stored in a desiccator for later use. 2.5480g AgNO3 was weighed and dissolved in water to form a solution with a silver ion concentration of 1.5mol / L, 1.4551g Co(NO3)2·6H2O was weighed and dissolved in water to form a solution with a cobalt ion concentration of 0.5mol / L, 1.0426g glycine was weighed and dissolved in 10mL deionized water and mixed with AgNO3 solution and Co(NO3)2·6H2O solution to form a mixed solution with a concentration of 3.3mol / L, wherein the molar ratio of silver ions to cobalt ions was 3:1, and the dried aluminum silicate filter membrane was immersed in the above mixed solution for 4h, and the excess liquid was drained by squeezing, dried at 80℃ for 10h, and placed in a box-type resistance furnace at 400℃ for 1h to obtain a silver / cobalt tetroxide / aluminum silicate filter membrane composite material. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of silver / cobalt oxide / aluminum silicate filter composite layer is 19%, and the catalyst loading is 0.0027 g / cm 3 .
[0074] See also Figure 2 , is the X-ray diffraction pattern of the silver / cobalt tetroxide / aluminum silicate filter membrane composite material prepared in Example 13 of the present invention, which shows that the prepared silver / cobalt tetroxide / aluminum silicate filter membrane composite material contains a silver phase and a cobalt tetroxide phase.
[0075] Embodiment 14
[0076] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 80℃ for 4h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a dryer for later use. Weigh 25.48g AgNO3 and dissolve it in water to form a solution with a silver ion concentration of 2.0mol / L. Then weigh 10.426g citric acid and dissolve it in 73mL deionized water and mix it with the AgNO3 solution to form a mixed solution with a concentration of 2.7mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 0.5h, and the excess liquid was drained by squeezing. It was dried at 100℃ for 24h and placed in a box-type resistance furnace at 500℃ for 10h to obtain a silver / aluminum silicate filter membrane composite material. The obtained composite material is complete and can be twisted at will without breaking or falling off. The loading of the silver / aluminum silicate filter composite layer is 62%, and the catalyst loading is 0.0097 g / cm 3 .
[0077] Embodiment 15
[0078] A 5mm thick aluminum silicate filter membrane (pore size 1μm-50μm) was cut into a circular filter disc with a diameter of 5cm, which was laid flat on tin foil and placed in a box-type resistance furnace. It was heat treated at 400℃ for 0.5h in an air atmosphere. The pretreated aluminum silicate filter membrane was sealed with tin foil and stored in a desiccator for later use. 14.551g Co(NO3)2·6H2O was weighed and dissolved in water to form a solution with a cobalt ion concentration of 2.0mol / L, and 10.426g urea was weighed and dissolved in 24mL deionized water and mixed with the Co(NO3)2·6H2O solution to form a mixed solution with a concentration of 9mol / L. The dried aluminum silicate filter membrane was immersed in the above mixed solution for 1h, and the excess liquid was drained by squeezing, dried at 100℃ for 2h, and placed in a box-type resistance furnace at 500℃ for 10h to obtain a cobalt oxide / aluminum silicate filter membrane composite material. The obtained composite material is complete and can be twisted at will without any breakage or slag. The loading of the cobalt oxide / aluminum silicate filter membrane composite layer is 75%, and the catalyst loading is 0.0120 g / cm 3 .
[0079] Example 16
[0080] This embodiment provides an air purification method, specifically, the aluminum silicate filter membrane-based composite material provided by the present invention is brought into contact with the gas to be purified. Specifically, an air purification device is provided: a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool, and the reaction process is:
[0081] (1) placing the aluminum silicate filter membrane composite material prepared in Examples 1 to 5 into a circular quartz tube container;
[0082] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump with an injection flow rate of 0.4 ul / min;
[0083] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0084] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0085] (5) The total flow rate was adjusted to 200 mL / min;
[0086] (6) The initial formaldehyde concentration is 3 ppm.
[0087] The manganese oxide / aluminum silicate filter membrane composite materials prepared in Examples 1 to 5 all have different degradation effects on formaldehyde. In this example, the concentration of the manganese nitrate aqueous solution was measured to be 0.8 mol / L through formaldehyde online detection and phenol reagent absorption method, with the highest catalytic activity and a formaldehyde conversion rate of 100%.
[0088] Table 1 Comparison of manganese nitrate concentration and formaldehyde degradation rate of aluminum silicate membrane-based composite materials in Examples 1-5
[0089]
[0090]
[0091] In Example 1, the manganese nitrate concentration is too high, resulting in an excessively high loading amount. The catalyst blocks the pores of the aluminum silicate filter membrane, increases wind resistance, decreases air permeability, and causes a decrease in the catalytic performance for formaldehyde.
[0092] Embodiment 17
[0093] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0094] (1) placing the manganese oxide / aluminum silicate filter membrane composite material prepared in Examples 4, 6, and 7 into a circular quartz tube container;
[0095] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump with an injection flow rate of 0.4 ul / min;
[0096] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0097] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0098] (5) The total flow rate was adjusted to 200 mL / min;
[0099] (6) The initial formaldehyde concentration is 3 ppm;
[0100] The manganese oxide / aluminum silicate filter membrane composite materials prepared in Examples 4, 6, and 7 all have different degradation effects on formaldehyde. In this example, the formaldehyde online detector and the phenol reagent absorption method measured that when the aluminum silicate filter membrane thickness was 5 mm, it was loaded with manganese oxide and had the highest catalytic activity, and the formaldehyde conversion rate was 91%.
[0101] Table 2 Comparison of aluminum silicate membrane thickness and formaldehyde degradation rate in Examples 4, 6, and 7
[0102] Example Aluminum silicate membrane thickness (mm) Formaldehyde degradation rate (%) Example 4 5 91 Example 6 2 42 Example 7 10 68
[0103] In order to measure the permeability of aluminum silicate filter membranes of different thicknesses, aluminum silicate filter membranes of different thicknesses were placed in the air purifier, and the wind speed of the gas was measured at the outlet using a wind resistance tester. The results are as follows:
[0104] Table 3 Comparison of permeability of different aluminum silicate membrane thicknesses
[0105] Aluminum silicate membrane thickness (mm) Power(W) Wind speed (m / s) 2 50.66 10.8 5 38.88 9.1 10 12.88 2.3
[0106] It can be seen from the test data that increasing the thickness of the filter membrane will increase wind resistance and affect the conversion efficiency of formaldehyde at room temperature.
[0107] Embodiment 18
[0108] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0109] (1) placing the manganese oxide / aluminum silicate filter membrane composite material prepared in Examples 4 and 8 into a circular quartz tube container;
[0110] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump with an injection flow rate of 0.4 ul / min;
[0111] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0112] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0113] (5) The total flow rate was adjusted to 200 mL / min;
[0114] (6) The initial formaldehyde concentration is 3 ppm;
[0115] The manganese oxide / aluminum silicate filter membrane composite materials prepared in Examples 4 and 8 have different degradation effects on formaldehyde. In this example, the composite material loaded with manganese oxide that removes excess liquid by extrusion has good catalytic activity, as measured by a formaldehyde online detector and a phenol reagent absorption method.
[0116] Table 4 Comparison of formaldehyde degradation rates of manganese oxide / aluminum silicate filter membrane composites prepared by different drainage methods
[0117] Example Drainage method Formaldehyde degradation rate (%) Example 4 extrusion 91 Example 8 Filtration 84
[0118] Embodiment 19
[0119] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0120] (1) placing the manganese oxide / aluminum silicate filter membrane composite material prepared in Examples 4 and 10 into a circular quartz tube container;
[0121] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump with an injection flow rate of 0.4 ul / min;
[0122] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0123] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0124] (5) The total flow rate was adjusted to 200 mL / min;
[0125] (6) The initial formaldehyde concentration is 3 ppm;
[0126] The manganese oxide / aluminum silicate filter membrane composite materials prepared in Examples 4 and 10 have different degradation effects on formaldehyde. In this example, the composite material loaded with manganese oxide prepared by the in-situ combustion method after drying has good catalytic activity, as measured by a formaldehyde online detector and a phenol reagent absorption method.
[0127] Table 5 Comparison of formaldehyde degradation rates of manganese oxide / aluminum silicate filter membrane composites prepared by different calcination methods
[0128]
[0129]
[0130] Embodiment 20
[0131] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0132] (1) placing the manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 into a circular quartz tube container;
[0133] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump, and the injection flow rate is 0.7ul / min;
[0134] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0135] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0136] (5) The total flow rate was adjusted to 200 mL / min;
[0137] (6) The initial formaldehyde concentration is 5 ppm;
[0138] (7) Conduct activity testing for one week
[0139] The manganese oxide / aluminum silicate filter membrane composite material prepared in Example 4 was tested for one week. The composite material loaded with manganese oxide / aluminum silicate filter membrane still maintained a degradation rate of 84% and had good catalytic stability as measured by the formaldehyde online detector and the phenol reagent absorption method in this example.
[0140] Embodiment 21
[0141] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0142] (1) placing the aluminum silicate filter membrane-based composite materials prepared in Examples 4, 11, 12, and 13 into a circular quartz tube container;
[0143] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump with an injection flow rate of 0.4 ul / min;
[0144] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0145] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0146] (5) The total flow rate was adjusted to 200 mL / min;
[0147] (6) The initial formaldehyde concentration is 3 ppm;
[0148] The aluminum silicate filter membrane-based composite materials prepared in Examples 4, 11, 12, and 13 all have different degradation effects on formaldehyde. In this example, the silver / cobalt tetroxide / aluminum silicate filter membrane composite material prepared by the in-situ combustion method was measured to have good catalytic activity through a formaldehyde online detector and a phenol reagent absorption method.
[0149] Table 6 Comparison of formaldehyde degradation rates of manganese oxide / aluminum silicate filter membrane composites prepared by different catalysts
[0150]
[0151]
[0152] Embodiment 22
[0153] The air purification device used in this embodiment is a cylindrical quartz container with an inner diameter of 5 cm and a volume of 98 mL filled with quartz wool. The reaction process is as follows:
[0154] (1) placing the silver / cobalt oxide / aluminum silicate filter membrane composite material prepared in Example 13 into a circular quartz tube container;
[0155] (2) Liquid formaldehyde is introduced into the pollutant generator through an injection pump, and the injection flow rate is 0.7ul / min;
[0156] (3) The pollutant generator gasifies the formaldehyde, and the gasification temperature is 103°C;
[0157] (4) The air generator inlet pressure is adjusted to 0.4 MPa;
[0158] (5) The total flow rate was adjusted to 200 mL / min;
[0159] (6) The initial formaldehyde concentration is 5 ppm;
[0160] (7) Conduct activity testing for one week
[0161] The silver / cobalt tetroxide / aluminum silicate filter membrane composite material prepared in Example 13 was tested for one week. The silver / cobalt tetroxide / aluminum silicate filter membrane composite material still maintained a degradation rate of 86% and had good catalytic stability as measured by the formaldehyde online detector and the phenol reagent absorption method in this example.
[0162] Comparative Example 1
[0163] The difference between this control example and all the embodiments is that no active component is immersed, and only an aluminum silicate filter membrane is used.
[0164] The aluminum silicate filter membrane prepared in this comparative example was used in Example 16, and the formaldehyde conversion rate was 11%.
[0165] Comparative Example 2
[0166] The difference between this control example and Example 4 is that the aluminum silicate filter membrane is immersed in the mixed solution for 24 hours.
[0167] The manganese oxide / aluminum silicate filter membrane composite material prepared in this comparative example was used in Example 16, and the formaldehyde conversion rate was 33%.
[0168] The soaking time will affect the loading amount of the catalyst. A long soaking time will make the filter membrane soft and difficult to shape and load the catalyst.
[0169] Comparative Example 3
[0170] The difference between this control example and Example 13 is that no reducing agent is added.
[0171] The silver / cobalt tetroxide / aluminum silicate filter membrane composite material prepared in this comparative example was used in Example 16, and the formaldehyde conversion rate was 52%.
[0172] Comparative Example 4
[0173] The difference between this control example and Example 4 is that the thickness of the aluminum silicate filter membrane is 1 mm.
[0174] The obtained composite material can be twisted at will without any slag falling off. However, after the catalyst is loaded on the 1mm aluminum silicate filter membrane, the periphery of the filter membrane becomes less smooth and slightly curved.
[0175] In summary, the present invention provides an aluminum silicate filter membrane-based composite material, including a substrate and a catalyst. The substrate is an aluminum silicate filter membrane with adsorption properties. The catalyst includes any one of elemental silver, manganese oxide, and cobalt tetroxide, or a mixture of two or more thereof. The catalyst is firmly attached to the surface and interior of the substrate and is not easy to fall off. The catalyst has a high loading content and is highly efficient when used to degrade formaldehyde.
[0176] The present invention also provides a method for preparing the material, comprising: providing a mixed solution containing manganese salt, silver salt, cobalt salt and a reducing agent, immersing an aluminum silicate filter membrane in the mixed solution, draining the remaining liquid, and performing heat treatment to obtain an aluminum silicate filter membrane-based composite material. Immersion time is a key factor, and too long or too short an immersion time will result in poor material performance.
[0177] The present invention also provides an air purification method, comprising bringing the aluminum silicate-based composite material provided by the present invention into contact with gas carrying polluted organic matter, and utilizing the catalyst loaded on the surface and inside of the aluminum silicate-based composite material to catalytically degrade the polluted organic matter, with high stability and high degradation efficiency.
[0178] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0179] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. An aluminum silicate filter membrane-based composite material, characterized in that: including a substrate and a catalyst; The substrate includes an aluminum silicate filter membrane; The catalyst comprises any one of elemental silver, manganese oxide, and cobalt tetraoxide, or a mixture of two or more thereof; The catalyst is attached to the surface and the interior of the substrate.
2. The aluminum silicate filter membrane-based composite material according to claim 1, characterized in that: The aluminum silicate filter membrane has a thickness of 2 mm to 10 mm and a pore size of 1 μm to 50 μm; And / or, the content of the catalyst in the aluminum silicate filter membrane-based composite material is 2.7% to 88%.
3. The aluminum silicate filter membrane-based composite material according to claim 1, characterized in that: The catalyst loading is 0.0001 g / cm 3 -0.02g / cm 3 .
4. The method for preparing the aluminum silicate filter membrane-based composite material according to any one of claims 1 to 3, characterized in that: include: An aqueous solution of any one of manganese salt, silver salt and cobalt salt or an aqueous solution of a combination of two or more of them is provided and mixed with a reducing agent to form a mixed solution, an aluminum silicate filter membrane is immersed in the mixed solution, and after the remaining liquid is discharged, heat treatment is performed to obtain an aluminum silicate filter membrane-based composite material.
5. The method for preparing the aluminum silicate filter membrane-based composite material according to claim 4, characterized in that Also includes: Before the aluminum silicate filter membrane is immersed in the mixed solution, the aluminum silicate filter membrane is pretreated, and the pretreatment includes treating the aluminum silicate filter membrane at 80-550° C. for 0.5-4 hours; And / or, the heat treatment includes heat treating the aluminum silicate filter membrane at 200-500° C. for 1-10 hours in an air atmosphere.
6. The method for preparing the aluminum silicate filter membrane-based composite material according to claim 5, characterized in that: The manganese salt includes any one of manganese nitrate, manganese sulfate, and manganese chloride, or a combination of two or more thereof; And / or, the silver salt includes any one of silver nitrate and silver fluoride or a combination of both; And / or, the cobalt salt comprises cobalt nitrate.
7. The method for preparing the aluminum silicate filter membrane-based composite material according to claim 6, characterized in that: The reducing agent includes any one of glycine, citric acid, and urea, or a combination of two or more thereof; And / or, the mass ratio of the reducing agent to any one or a combination of two or more of the mixed manganese salt, silver salt, and cobalt salt is 1:4-12.
8. The preparation method according to claim 4, characterized in that: The aluminum silicate filter membrane is immersed in the mixed solution for 0.5-24h; And / or, before the heat treatment, the aluminum silicate filter membrane is dried at 80-100° C. for 10-24 hours.
9. The preparation method according to claim 8, characterized in that: The concentration of manganese ions in the aqueous solution of the manganese salt is 0.06 mol / L-3.5 mol / L; and / or, the concentration of silver ions in the aqueous solution of the silver salt is 0.3 mol / L-2 mol / L; And / or, the concentration of cobalt ions in the aqueous solution of the cobalt salt is 0.1 mol / L-2 mol / L.
10. An air purification method, characterized in that: The method comprises at least bringing the aluminum silicate filter membrane-based composite material as described in any one of claims 1 to 3 into contact with a gas containing formaldehyde, wherein the formaldehyde concentration is 3 to 10 ppm.
11. Use of the aluminum silicate filter membrane-based composite material as described in any one of claims 1 to 3, or the aluminum silicate filter membrane-based composite material prepared by the method as described in any one of claims 4 to 8, or the air purification method as described in claim 9 in degrading pollutants.
Citation Information
Patent Citations
Method for preparing filtering-catalysis integrated porous film
CN108339413A
Formaldehyde oxidation composite catalytic material and preparation method thereof
CN109759080A
Manganese oxide-activated carbon composite catalyst as well as preparation method and application thereof
CN109926044A
Porous nano manganese oxide catalyst, preparation and application thereof
CN110404530A
Ceramic fiber catalytic filter element and integrated preparation method thereof
CN110694353A