Composite photocatalyst as well as preparation method and application thereof
By loading TixCuyOz clusters on MoS2 nanosheets and calcining to remove organic ligands, the problems of easy stacking and limited active sites of MoS2 nanosheets are solved, significantly improving the photocatalytic hydrogen evolution efficiency, and achieving efficient photocatalytic and clean energy utilization.
Patent Information
- Application Number
- CN202410997041.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-12-03
AI Technical Summary
MoS2 nanosheets are prone to stacking and have limited active sites in photocatalytic applications, which limits the improvement of their catalytic performance. The surface organic ligand coating of metal clusters will mask active sites and affect catalytic performance.
Develop a composite photocatalyst of TixCuyOz clusters and MoS2 nanosheets. By loading TixCuyOz clusters onto MoS2 nanosheets, the active sites are exposed using the precise structure and stability of the clusters to improve photocatalytic activity, and the organic ligands are removed through calcination. Enhance interface contact.
The photocatalytic hydrogen evolution efficiency is significantly improved, with hydrogen evolution efficiency as high as 5531.7μmol·g-1·h-1, making up for the insufficient active sites of MoS2 nanosheets, and providing efficient industrial application photocatalysts and low-cost clean energy utilization solutions.
Smart Images

Figure CN119056468A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of novel hydrogen energy conversion, in particular to Ti x Cu y O z Clusters and MoS 2 Nanosheet composite photocatalyst, preparation method and application thereof. Background Art
[0002] With the continuous development of the global economy and the continuous growth of population, the demand for energy has increased dramatically, while the over-exploitation and utilization of traditional fossil energy such as oil and coal are facing the severe challenge of resource depletion. More seriously, the large amount of greenhouse gases released during the combustion of these energy sources, such as carbon dioxide, have aggravated the global greenhouse effect, leading to a series of environmental problems such as climate change, melting glaciers, rising sea levels and damage to biodiversity, which urgently requires humans to find and develop clean and sustainable alternative energy.
[0003] As an ideal clean energy, hydrogen energy is regarded as an important component of the future energy system because its combustion product is only water, no pollutants are emitted, and it has high energy density. However, the widespread application of hydrogen energy is limited by its efficient and economical preparation technology. Among the many hydrogen production methods, solar photocatalytic hydrogen production has become a research hotspot because of its green and renewable characteristics. This method uses solar energy to drive the water decomposition reaction to directly generate hydrogen and oxygen, which has the advantages of low cost, environmental friendliness, and strong sustainability.
[0004] In the field of photocatalytic hydrogen production, two-dimensional transition metal sulfides (TMDs), especially molybdenum disulfide (MoS 2 ) nanosheets, due to their unique two-dimensional layered structure, good optoelectronic properties and low preparation cost, have shown great application potential. MoS 2 Nanosheets can not only act as independent photocatalysts, but also as carriers and composites with other materials to improve photocatalytic efficiency. 2 In practical applications, nanosheets face problems such as easy accumulation and limited active sites, which restricts the improvement of their catalytic performance.
[0005] To solve the above problems, researchers tried to 2 Metal nanoparticles are loaded on nanosheets to improve photocatalytic activity by changing their electronic structure and promoting charge separation. However, the polydispersity of nanoparticles makes it difficult to precisely control the surface electronic structure and explore the photocatalytic reaction mechanism in depth. In contrast, metal clusters have become an ideal model for studying structure-activity relationships due to their precise atomic structure and clear crystal structure. By anchoring precious metal clusters such as Au, Ag, Pt, and Pd on MoS 2Nanosheets not only effectively inhibit the MoS 2 The charge transfer efficiency is significantly improved.
[0006] Clusters, as a bridge between molecules and nanoparticles or bulk materials, exhibit unique intrinsic properties. Compared with nanoparticles, clusters have two significant advantages: first, through advanced characterization techniques such as X-ray diffraction, we can accurately obtain the structural information of these crystalline materials, and these data provide a solid and precise foundation for in-depth theoretical calculations and mechanism interpretations; second, clusters stabilized by organic ligands can be easily dissolved in organic solvents, which is convenient for recrystallization and post-functionalization treatment, and is the key cornerstone for the bottom-up assembly strategy of a variety of new functional materials. Therefore, these molecular materials with highly consistent composition, size and shape effectively overcome the structural inaccuracy and inhomogeneity of nanoparticle materials. It is particularly worth mentioning that polyoxometalates (POMs), as a typical representative of the cluster family, have not only set a model for the bottom-up assembly method of cluster-based composite materials, but also demonstrated excellent performance in a wide range of applications.
[0007] Although metal clusters have shown many advantages in the field of photocatalysis, the coating of organic ligands on their surfaces may shield the active sites, hindering the effective participation of photogenerated electrons, and thus affecting the catalytic performance. Therefore, how to maximize the exposure of active sites while maintaining the stability of the cluster structure has become a major challenge in current research. Summary of the invention
[0008] Aiming at the shortcomings of existing technologies, we develop efficient and stable MoS 2 Based photocatalyst, overcoming MoS 2 Nanosheets are easy to accumulate, have limited active sites, and at the same time make full use of the advantages of metal clusters to achieve efficient conversion of solar energy to hydrogen energy. The present invention provides Ti x Cu y O z Clusters and MoS 2 Nanosheet composite photocatalyst, preparation method and application thereof.
[0009] The first aspect of the present invention is to provide Ti x Cu y O z Clusters and MoS 2 The preparation method of the composite photocatalyst of nanosheets comprises the following steps:
[0010] Provide Ti x Cu y O z NCs (titanium copper oxygen nanoclusters);
[0011] Provide MoS 2 NSs (MoS2 nanosheets);
[0012] MoS 2 NSs load to Ti x Cu y O z NCs, Ti x Cu y O z Clusters and MoS 2 Composite photocatalysts of nanosheets;
[0013] Among them, x and z are both positive numbers, and y is a number ≥0.
[0014] Preferably, the Ti x Cu y O z Clusters and MoS 2 The composite photocatalyst of nanosheets was also calcined.
[0015] In a preferred embodiment, x is a positive number of 1-10, preferably 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.
[0016] In a preferred embodiment, y is a number from 0 to 10, preferably a positive integer from 1 to 10, preferably 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.
[0017] In a preferred embodiment, z is a positive number of 1-10, preferably 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.
[0018] In a preferred embodiment, the Ti x Cu y O z The preparation method of NCs comprises the following steps:
[0019] providing a copper precursor;
[0020] The copper precursor, benzoic acid, triethylamine and isopropyl titanate are mixed and reacted in a first solvent to obtain Ti x Cu y O z NCs.
[0021] In a preferred embodiment, the method for preparing the copper precursor comprises the following steps:
[0022] Cu 2 O (cuprous oxide), tetrafluoroboric acid and a cyano (-CN)-containing compound are mixed and reacted to obtain [Cu(CH 3 CN) 4]BF 4 , i.e., copper precursor.
[0023] Preferably, the cyano group-containing compound is selected from one or more of acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide and chloroacetonitrile.
[0024] Preferably, Cu 2 The reaction temperature of O, tetrafluoroboric acid and the cyano group-containing compound is 50-100°C, preferably 60-80°C, more preferably 70-75°C.
[0025] Preferably, Cu 2 The reaction time of O, tetrafluoroboric acid and the cyano group-containing compound is 5-80 min, preferably 8-60 min, and more preferably 10-30 min.
[0026] Preferably, Cu 2 O, tetrafluoroboric acid, and a cyano-containing compound, the steps comprising:
[0027] Add tetrafluoroboric acid to Cu 2 O and a cyano-containing compound in a mixed solution.
[0028] More preferably, tetrafluoroboric acid is added to the Cu 2 Before mixing the solution of CuO with the cyano compound, the Cu 2 The temperature of the mixed solution of O and the cyano group-containing compound is 50-100°C, preferably 60-80°C, more preferably 70-75°C.
[0029] Preferably, Cu 2 After the reaction of O, tetrafluoroboric acid and cyano-containing compounds is completed, cooling and crystallization are required to obtain a copper precursor.
[0030] More preferably, the temperature of the cooling crystallization is -15-5°C, preferably -10-3°C, more preferably -5-0°C.
[0031] More preferably, the cooling crystallization time is 5-24 h, preferably 8-16 h, more preferably 10-12 h.
[0032] More preferably, after the cooling crystallization, post-treatment is performed.
[0033] More preferably, the post-treatment comprises washing.
[0034] Preferably, Cu 2 O, tetrafluoroboric acid, and a cyano-containing compound, wherein the cleaning solvent used for cleaning is one or more of water, ethanol, and methanol.
[0035] Preferably, Cu 2After the reaction product of O, tetrafluoroboric acid and the cyano group-containing compound is cleaned, it is also necessary to dry it.
[0036] More preferably, Cu 2 The drying method of the reaction product of O, tetrafluoroboric acid and the cyano group-containing compound is freeze-drying.
[0037] Preferably, the first solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.
[0038] Preferably, the reaction temperature of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is 50-100°C, preferably 60-90°C, and more preferably 70-80°C.
[0039] Preferably, the reaction time of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is 12-72 h, preferably 24-60 h, and more preferably 36-48 h.
[0040] Preferably, the reaction product of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is also cleaned.
[0041] More preferably, the reaction product of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is cleaned with a cleaning solvent selected from the group consisting of water, ethanol and methanol.
[0042] Preferably, the reaction product of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is dried after cleaning.
[0043] More preferably, the reaction product of the copper precursor, benzoic acid, triethylamine and isopropyl titanate has a drying temperature of 50-100°C, preferably 55-80°C, and more preferably 60-75°C.
[0044] More preferably, the drying time of the reaction product of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is 4-24 h, preferably 6-18 h, and more preferably 8-12 h.
[0045] In a preferred embodiment, the MoS 2 The preparation method of NSs comprises the following steps:
[0046] Ammonium molybdate (NH 4 ) 6 Mo7 O 24 ), the sulfur source is mixed and reacted in the second solvent to obtain MoS 2 NSs.
[0047] In a preferred embodiment, the sulfur source includes thioacetamide (TAA), thiourea (CH 4 N 2 S), one or more combinations of mercaptans and thioethers.
[0048] Preferably, the (NH 4 ) 6 Mo 7 O 24 It can be provided in the form of a hydrate, an aqueous solution or an alcohol solution.
[0049] Preferably, the second solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.
[0050] Preferably, the reaction temperature of the ammonium molybdate and the sulfur source is 180-300°C, preferably 210-240°C, more preferably 220-230°C.
[0051] Preferably, the reaction time of the ammonium molybdate and the sulfur source is 5-24 h, preferably 8-20 h, and more preferably 10-18 h.
[0052] Preferably, the reaction product of ammonium molybdate and sulfur source is also cleaned.
[0053] More preferably, the reaction product of ammonium molybdate and the sulfur source is washed with a cleaning solvent selected from the group consisting of water, ethanol and methanol.
[0054] Preferably, the reaction product of ammonium molybdate and sulfur source is dried after washing.
[0055] More preferably, the drying temperature of the reaction product of ammonium molybdate and sulfur source is 50-100°C, preferably 55-80°C, more preferably 60-75°C.
[0056] More preferably, the drying time of the reaction product of ammonium molybdate and sulfur source is 8-48 h, preferably 12-36 h, more preferably 16-24 h.
[0057] In a preferred embodiment, the MoS 2 NSs load to Ti x Cu y O z NCs, the steps include: 2 NSs、Ti x Cu y O z The NCs are mixed in a third solvent.
[0058] Preferably, the third solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.
[0059] Preferably, MoS 2 NSs、Ti x Cu y O z Before mixing the NCs in the third solvent, the MoS 2 NSs was added to the third solvent and mixed to obtain MoS 2 NSs solution;
[0060] Ti x Cu y O z NCs are added to the third solvent and mixed to obtain Ti x Cu y O z NCs solution.
[0061] More preferably, Ti x Cu y O z NCs solution was added dropwise to MoS 2 NSs solution to obtain an intermediate product.
[0062] Preferably, the intermediate product is further cleaned.
[0063] More preferably, the intermediate product is washed with one or more of the following cleaning solvents: water, ethanol, methanol, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, and chloroacetonitrile.
[0064] Preferably, the intermediate product is dried after cleaning.
[0065] More preferably, the intermediate product has a drying temperature of 50-100°C, preferably 55-80°C, more preferably 60-75°C.
[0066] More preferably, the intermediate product has a drying time of 8-48 h, preferably 10-36 h, and more preferably 12-24 h.
[0067] Preferably, MoS 2 NSs load to Ti x Cu y O z NCs, whose MoS 2 NSs、Ti x Cu y O z The material ratio (mass ratio) of NCs is 1:(1-20), preferably 1:(1-15), and more preferably 1:(1-10).
[0068] In a preferred embodiment, the calcination temperature of the intermediate product is set according to its thermogravimetric curve. Specifically, the calcination temperature is the temperature at which the organic ligand is completely removed.
[0069] Preferably, the calcination temperature is not lower than the "residual mass stabilization temperature" of the thermogravimetric curve.
[0070] Preferably, the calcination atmosphere is an inert gas, preferably one or more of nitrogen, helium and argon.
[0071] A second aspect of the present invention is to provide Ti x Cu y O z Clusters and MoS 2 A composite photocatalyst of nanosheets, wherein x and z are both positive numbers, and y is a number ≥0.
[0072] Preferably, in Ti x Cu y O z Clusters and MoS 2 In the composite photocatalyst of nanosheets, Ti x Cu y O z With MoS 2 The mass ratio is 1:(1-20), preferably 1:(1-15), and more preferably 1:(1-10).
[0073] Preferably, in Ti x Cu y O z Clusters and MoS 2 In the composite photocatalyst of nanosheets, the structure is Ti x Cuy O z Cluster@MoS 2 Nanosheets, namely MoS 2 Nanosheets wrapped Ti x Cu y O z Clusters.
[0074] Preferably, the Ti x Cu y O z Clusters and MoS 2 The composite photocatalyst of nanosheets is obtained based on the aforementioned preparation method.
[0075] The third aspect of the present invention is to provide Ti x Cu y O z Clusters and MoS 2 Application of composite photocatalyst of nanosheets, the composite photocatalyst can be applied to water electrolysis catalyst, especially hydrogen evolution catalyst.
[0076] In the present application, the residual mass stabilization temperature is the temperature on the thermogravimetric curve at which the mass of the sample no longer changes significantly with increasing temperature. This indicates that the volatile components, decomposable components, etc. in the sample have all been lost or decomposed. At this time, the mass of the sample remains relatively stable, and the corresponding temperature is the residual mass stabilization temperature.
[0077] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0078] The present invention provides Ti x Cu y O z Clusters and MoS 2 Nanosheet composite photocatalyst, its preparation method and application, through a mild one-step hydrothermal reaction, coagulation precipitation, and high-temperature calcination, the semiconductor material---Ti is efficiently synthesized. x Cu y O z Clusters and MoS 2 Composite photocatalysts of nanosheets.
[0079] Due to the enhanced absorption of visible light by the composite photocatalyst of the present invention and the effective separation of photogenerated holes and electrons, it exhibits excellent photocatalytic hydrogen evolution activity for water splitting and hydrogen evolution, which also indicates that Ti x Cu y O z The clusters were successfully loaded onto MoS 2The nanosheets are bonded to form a heterojunction with them, providing more active sites for the composite material, significantly improving its photocatalytic hydrogen evolution efficiency and making up for the MoS 2 The disadvantage of nanosheets is that they have few active sites.
[0080] The hydrogen evolution efficiency of the composite photocatalyst of the present invention is as high as 5531.7 μmol·g -1 ·h -1 The total amount of hydrogen evolution in the first 12 hours even reached 53764.4 μmol·g-1. The present invention provides a new approach for further designing efficient industrial photocatalysts and also provides a new solution for low-cost sustainable utilization of clean energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0081] Figure 1 Ti obtained in Example 2 of the present invention 4 Cu 2 O nanoclusters and Ti 4 Cu 2 O NCs / MoS 2 Thermogravimetric analysis curves of NSs nanocomposites.
[0082] Figure 2 The composite material Ti obtained in Example 2 of the present invention 4 Cu 2 O / MoS 2 Transmission electron microscope image and dark field image of (MT-5A).
[0083] Figure 3 (The vertical axis is the hydrogen evolution rate H 2 evolution rate) is the single component Ti-O, Ti obtained in Examples 1-4 of the present invention 4 Cu 2 O NCs, MoS 2 NSs and composite Ti-O NCs / MoS 2 NSs(MT-0),Ti 4 Cu 2 O NCs / MoS 2 Hydrogen evolution efficiency of NSs (MT-1, MT-5, MT-10) under (a) different sacrificial agents, (b) annealing or not, (c) the change trend of hydrogen evolution efficiency and total hydrogen production (including MT-5A) after 12 h of continuous reaction, and (d) the cyclic test of sample MT-5A during 60 h of reaction.
[0084] Figure 4 Ti obtained in Examples 2 and 4 of the present invention x Cu y O z Clusters, MoS 2Nanosheets, Ti 4 Cu 2 O / MoS 2 Nanocomposites (MT-5A) and Ti-O NCs / MoS 2 (a) Photoresponse current (time on the horizontal axis, current on the vertical axis); (b) electrochemical impedance spectroscopy; (c) photoluminescence spectrum (wavelength on the horizontal axis, intensity on the vertical axis) of NSs nanocomposite material (MT-0A). DETAILED DESCRIPTION
[0085] The embodiment of the present invention provides Ti x Cu y O z Clusters and MoS 2 Nanosheet composite photocatalyst, preparation method thereof and application thereof, in order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0086] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0087] Example 1
[0088] (1) Titanium copper oxide nanoclusters (Ti 4 Cu 2 Preparation of O NCs:
[0089] (i) Copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) synthesis: The specific steps are as follows: 1 gram (g) of cuprous oxide (Cu 2 O) and 250 ml (mL) of acetonitrile were placed in a round-bottom flask, and then the round-bottom flask was placed in an oil bath and kept warm at 70°C; after 3-5 minutes (min) of magnetic stirring, 5 mL of tetrafluoroboric acid was added, and then magnetic stirring was continued for another 10-15 minutes until the mixed solution was completely clarified.
[0090] The round-bottom flask containing the 70°C hot solution was sealed and quickly placed in a refrigerator to quickly cool it to about 0°C; after 12 hours (h) of low-temperature refrigeration, a large amount of white crystals precipitated at the bottom of the flask. After centrifugation and alcohol washing 2-3 times, the precipitated crystals were freeze-dried, and the final white crystals were the copper precursor.
[0091] (ii) Preparation of titanium copper oxide nanoclusters: 1.5 g of benzoic acid and 43.5 g of copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) in a beaker, and then add 8 mL of acetonitrile and 120 μL of triethylamine (C 6 H 15 N) and 400 μL of isopropyl titanate (C 12 H 28 O 4 Ti), fully stirred and placed in an oven at 80°C, kept warm for two days, taken out, washed with acetonitrile 3-4 times and centrifuged, and finally placed in a vacuum drying oven at 60°C for drying for 12h.
[0092] (2) Molybdenum disulfide nanosheets (MoS 2 Preparation of NSs:
[0093] (i) Take 1 mmol of ammonium molybdate tetrahydrate (NH 4 ) 6 Mo 7 O 24 ·4H 2 O and 30 mmol thiourea (CH 4 N 2 S), dissolved in 35 mL of deionized water, and stirred vigorously to obtain a clear solution.
[0094] (ii) Then, the solution was poured into a 50 mL polytetrafluoroethylene-lined reactor, and the reactor was placed in an oven for hydrothermal reaction. The reaction temperature was set to 220°C and the reaction time was 18 hours. After the reaction was completed, the reactor was placed at room temperature to cool naturally, and the precipitate was collected and repeatedly washed with deionized water and anhydrous ethanol and centrifuged for several times; finally, the obtained separated product was placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain molybdenum disulfide nanosheets.
[0095] (3) MoS2 nanosheets loaded with titanium copper oxide nanoclusters (Ti 4 Cu 2 O NCs / MoS 2 Preparation of NSs:
[0096] (i) 50 mg MoS 2The nanosheets were dispersed in 50 mL of dichloromethane and sonicated for about 20-30 min to obtain a well-dispersed suspension.
[0097] (ii) Take 2.5 mg of Ti 4 Cu 2 O nanoclusters were dispersed in 2 ml of dichloromethane and ultrasonicated for about 30-40 min until the suspension was clear. 4 Cu 2 The clear dichloromethane solution of O nanoclusters was added dropwise to the ultrathin MoS 2 In the nanosheet dispersion, due to the ultrafine Ti 4 Cu 2 O nanoclusters have high surface energy, and MoS 2 After the nanosheets were combined, MoS was self-assembled through electrostatic forces. 2 Nanosheets on Ti 4 Cu 2 The loading on the O nanoclusters. During this process, the addition should be continued while stirring, and the stirring should be continued for 1 hour after the addition is completed. Finally, the fully stirred solution was centrifuged, washed with acetonitrile and anhydrous ethanol solution for 3-4 times, and then placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain Ti 4 Cu 2 O NCs / MoS 2 NSs nanocomposites.
[0098] Given that Ti 4 Cu 2 O and MoS 2 The material ratio has a great influence on the subsequent morphology construction and performance of the composite. In this embodiment, MoS 2 Nanosheets and Ti 4 Cu 2 The mass addition ratio of O nanoclusters is 1 / 1, abbreviated as MT-1.
[0099] (iii) Calcination: Considering Ti 4 Cu 2 The coating of organic ligands on the surface of O nanoclusters will hinder their bonding with MoS 2 Nanosheet charge transport, we prepared Ti 4 Cu 2 O NCs / MoS 2 The NSs nanocomposites were annealed and calcined to remove their surface ligands and further strengthen the interfacial contact between the two.
[0100] In order to judge Ti 4 Cu 2In this embodiment, all samples were calcined under nitrogen protection. The specific temperature was determined according to the thermogravimetric curve, which was the residual mass stabilization temperature on the thermogravimetric curve. The calcined Ti 4 Cu 2 O / MoS 2 The composite material is abbreviated as MT-1A.
[0101] Example 2
[0102] (1) Titanium copper oxide nanoclusters (Ti 4 Cu 2 Preparation of O NCs:
[0103] (i) Copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) synthesis: The specific steps are as follows: 1 gram (g) of cuprous oxide (Cu 2 O) and 250 ml (mL) of acetonitrile were placed in a round-bottom flask, and then the round-bottom flask was placed in an oil bath and kept warm at 70°C; after 3-5 minutes (min) of magnetic stirring, 5 mL of tetrafluoroboric acid was added, and then magnetic stirring was continued for another 10-15 minutes until the mixed solution was completely clarified.
[0104] The round-bottom flask containing the 70°C hot solution was sealed and quickly placed in a refrigerator to quickly cool it to about 0°C; after 12 hours (h) of low-temperature refrigeration, a large amount of white crystals precipitated at the bottom of the flask. After centrifugation and alcohol washing 2-3 times, the precipitated crystals were freeze-dried, and the final white crystals were the copper precursor.
[0105] (ii) Preparation of titanium copper oxide nanoclusters: 1.5 g of benzoic acid and 43.5 g of copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) in a beaker, and then add 8 mL of acetonitrile and 120 μL of triethylamine (C 6 H 15 N) and 400 μL of isopropyl titanate (C 12 H 28 O 4 Ti), fully stirred and placed in an oven at 80°C, kept warm for two days, taken out, washed with acetonitrile 3-4 times and centrifuged, and finally placed in a vacuum drying oven at 60°C for drying for 12h.
[0106] (2) Molybdenum disulfide nanosheets (MoS 2 Preparation of NSs:
[0107] (i) Take 1 mmol of ammonium molybdate tetrahydrate (NH4 ) 6 Mo 7 O 24 ·4H 2 O and 30 mmol thiourea (CH 4 N 2 S), dissolved in 35 mL of deionized water, and stirred vigorously to obtain a clear solution.
[0108] (ii) Then, the solution was poured into a 50 mL polytetrafluoroethylene-lined reactor, and the reactor was placed in an oven for hydrothermal reaction. The reaction temperature was set to 220°C and the reaction time was 18 hours. After the reaction was completed, the reactor was placed at room temperature to cool naturally, and the precipitate was collected and repeatedly washed with deionized water and anhydrous ethanol and centrifuged for several times; finally, the obtained separated product was placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain molybdenum disulfide nanosheets.
[0109] (3) MoS2 nanosheets loaded with titanium copper oxide nanoclusters (Ti 4 Cu 2 O NCs / MoS 2 Preparation of NSs:
[0110] (i) 50 mg MoS 2 The nanosheets were dispersed in 50 mL of dichloromethane and sonicated for about 20-30 min to obtain a well-dispersed suspension.
[0111] (ii) Take 2.5 mg of Ti 4 Cu 2 O nanoclusters were dispersed in 2 ml of dichloromethane and ultrasonicated for about 30-40 min until the suspension was clear. 4 Cu 2 The clear dichloromethane solution of O nanoclusters was added dropwise to the ultrathin MoS 2 In the nanosheet dispersion, due to the ultrafine Ti 4 Cu 2 O nanoclusters have high surface energy, and MoS 2 After the nanosheets were combined, MoS was self-assembled through electrostatic forces. 2 Nanosheets on Ti 4 Cu 2 The loading on the O nanoclusters. During this process, the addition should be continued while stirring, and the stirring should be continued for 1 hour after the addition is completed. Finally, the fully stirred solution was centrifuged, washed with acetonitrile and anhydrous ethanol solution for 3-4 times, and then placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain Ti 4 Cu 2 O NCs / MoS 2 NSs nanocomposites.
[0112] In this embodiment, MoS 2 Nanosheets and Ti 4 Cu 2 The mass addition ratio of O nanoclusters is 1 / 5, abbreviated as MT-5.
[0113] (iii) Calcination: Considering Ti 4 Cu 2 The coating of organic ligands on the surface of O nanoclusters will hinder their bonding with MoS 2 Nanosheet charge transport, we prepared Ti 4 Cu 2 O NCs / MoS 2 The NSs nanocomposites were annealed and calcined to remove their surface ligands and further strengthen the interfacial contact between the two.
[0114] In order to judge Ti 4 Cu 2 In this example, the sample was calcined under nitrogen protection. The specific temperature was determined according to the thermogravimetric curve, which was the residual mass stabilization temperature on the thermogravimetric curve. The calcined Ti 4 Cu 2 O / MoS 2 The composite material is abbreviated as MT-5A.
[0115] Example 3
[0116] (1) Titanium copper oxide nanoclusters (Ti 4 Cu 2 Preparation of O NCs:
[0117] (i) Copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) synthesis: The specific steps are as follows: 1 gram (g) of cuprous oxide (Cu 2 O) and 250 ml (mL) of acetonitrile were placed in a round-bottom flask, and then the round-bottom flask was placed in an oil bath and kept warm at 70°C; after 3-5 minutes (min) of magnetic stirring, 5 mL of tetrafluoroboric acid was added, and then magnetic stirring was continued for another 10-15 minutes until the mixed solution was completely clarified.
[0118] The round-bottom flask containing the 70°C hot solution was sealed and quickly placed in a refrigerator to quickly cool it to about 0°C; after 12 hours (h) of low-temperature refrigeration, a large amount of white crystals precipitated at the bottom of the flask. After centrifugation and alcohol washing 2-3 times, the precipitated crystals were freeze-dried, and the final white crystals were the copper precursor.
[0119] (ii) Preparation of titanium copper oxide nanoclusters: 1.5 g of benzoic acid and 43.5 g of copper precursor ([Cu(CH 3 CN) 4 ]BF 4 ) in a beaker, and then add 8 mL of acetonitrile and 120 μL of triethylamine (C 6 H 15 N) and 400 μL of isopropyl titanate (C 12 H 28 O 4 Ti), fully stirred and placed in an oven at 80°C, kept warm for two days, taken out, washed with acetonitrile 3-4 times and centrifuged, and finally placed in a vacuum drying oven at 60°C for drying for 12h.
[0120] (2) Molybdenum disulfide nanosheets (MoS 2 Preparation of NSs:
[0121] (i) Take 1 mmol of ammonium molybdate tetrahydrate (NH 4 ) 6 Mo 7 O 24 ·4H 2 O and 30 mmol thiourea (CH 4 N 2 S), dissolved in 35 mL of deionized water, and stirred vigorously to obtain a clear solution.
[0122] (ii) Then, the solution was poured into a 50 mL polytetrafluoroethylene-lined reactor, and the reactor was placed in an oven for hydrothermal reaction. The reaction temperature was set to 220°C and the reaction time was 18 hours. After the reaction was completed, the reactor was placed at room temperature to cool naturally, and the precipitate was collected and repeatedly washed with deionized water and anhydrous ethanol and centrifuged for several times; finally, the obtained separated product was placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain molybdenum disulfide nanosheets.
[0123] (3) MoS2 nanosheets loaded with titanium copper oxide nanoclusters (Ti 4 Cu 2 O NCs / MoS 2 Preparation of NSs:
[0124] (i) 50 mg MoS 2 The nanosheets were dispersed in 50 mL of dichloromethane and sonicated for about 20-30 min to obtain a well-dispersed suspension.
[0125] (ii) Take 2.5 mg of Ti 4 Cu 2 O nanoclusters were dispersed in 2 ml of dichloromethane and ultrasonicated for about 30-40 min until the suspension was clear.4 Cu 2 The clear dichloromethane solution of O nanoclusters was added dropwise to the ultrathin MoS 2 In the nanosheet dispersion, due to the ultrafine Ti 4 Cu 2 O nanoclusters have high surface energy, and MoS 2 After the nanosheets were combined, MoS was self-assembled through electrostatic forces. 2 Nanosheets on Ti 4 Cu 2 The loading on the O nanoclusters. During this process, the addition should be continued while stirring, and the stirring should be continued for 1 hour after the addition is completed. Finally, the fully stirred solution was centrifuged, washed with acetonitrile and anhydrous ethanol solution for 3-4 times, and then placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain Ti 4 Cu 2 O NCs / MoS 2 NSs nanocomposites.
[0126] In this embodiment, MoS 2 Nanosheets and Ti 4 Cu 2 The mass addition ratio of O nanoclusters is 1 / 10, abbreviated as MT-10.
[0127] (iii) Calcination: Considering Ti 4 Cu 2 The coating of organic ligands on the surface of O nanoclusters will hinder their bonding with MoS 2 Nanosheet charge transport, we prepared Ti 4 Cu 2 O NCs / MoS 2 The NSs nanocomposites were annealed and calcined to remove their surface ligands and further strengthen the interfacial contact between the two.
[0128] In order to judge Ti 4 Cu 2 In this example, the sample was calcined under nitrogen protection. The specific temperature was determined according to the thermogravimetric curve, which was the residual mass stabilization temperature on the thermogravimetric curve. The calcined Ti 4 Cu 2 O / MoS 2 The composite material is abbreviated as MT-10A.
[0129] Example 4
[0130] In order to determine the effect of the presence or absence of Cu atoms on the performance of the hydrogen evolution reaction, we synthesized Ti-O clusters without Cu atoms and combined them with MoS 2Nanosheets are composited, called Ti-O NCs / MoS 2 NSs (i.e. MT-0).
[0131] (1) Preparation of undoped copper titanium oxide nanoclusters (Ti-O NCs): 1.5 g of benzoic acid was placed in a beaker, and 8 mL of acetonitrile and 120 μL of triethylamine (C 6 H 15 N) and 400 μL of isopropyl titanate (C 12 H 28 O 4 After being fully stirred, the mixture was placed in an oven at 80°C for two days, taken out, washed with acetonitrile for 3-4 times and centrifuged, and finally placed in a vacuum drying oven at 60°C for 12 h to obtain titanium oxide nanoclusters, which were abbreviated as MT-0.
[0132] (2) In order to determine the effect of organic ligands in Ti-O NCs on hydrogen evolution performance, the samples were calcined under nitrogen protection in this example. The specific temperature was determined according to the thermogravimetric curve, which was the residual mass stabilization temperature on the thermogravimetric curve. The calcined Ti-O / MoS 2 The composite material is abbreviated as MT-0A.
[0133] Figure 1-4 The performance of the composite materials of Examples 1-4 was characterized and analyzed as follows:
[0134] Figure 1 The Ti obtained in Example 2 of the present invention is presented 4 Cu 2 O nanoclusters and Ti 4 Cu 2 O NCs / MoS 2 Thermogravimetric analysis curves of NSs nanocomposites.
[0135] In order to determine the appropriate calcination temperature, Ti 4 Cu 2 O nanoclusters and Ti 4 Cu 2 O NCs / MoS 2 Thermogravimetric analysis experiments were carried out on NSs nanocomposites. The specific experimental conditions are as follows: 4 Cu 2 O nanoclusters 4.433 mg and Ti 4 Cu 2 O NCs / MoS 2 2.785 mg of NSs nanocomposite material, the heating rate was set to 25 / 10.0 K / min, and the atmosphere was nitrogen (N 2 ), using open alumina (Al 2 O3 ) crucible, the measured thermogravimetric curves (TG) and thermogravimetric differential curves (DTG) of the two are as follows Figure 1 .
[0136] according to Figure 1 As shown in (a), when the temperature reaches about 320°C, Ti 4 Cu 2 O nanoclusters begin to lose weight, and the DTG curve shows that there is an obvious exothermic reaction in this area, which may be caused by Ti 4 Cu 2 Some weak ligands in O (such as isopropanol) decomposed. When the temperature continued to rise to 470 ° C, another weight loss reaction occurred, which may be due to the decomposition of strong ligands (such as benzoic acid). When it reached 500 ° C, there was basically no weight loss, and the composite material was similar ( Figure 1 b).
[0137] In order to completely remove the organic ligands, the calcination temperature in Examples 1-4 was determined to be 500°C.
[0138] The composite material after annealing and calcination is referred to as Ti 4 Cu 2 O / MoS 2 Composite materials.
[0139] Figure 2 The composite material Ti obtained in Example 2 of the present invention is presented 4 Cu 2 O / MoS 2 Transmission electron microscope image and dark field image of the composite material (MT-5A). 4 Cu 2 O / MoS 2 The microstructure of the composite materials was tested by transmission electron microscopy (TEM).
[0140] like Figure 2 As shown in the figure, it can be clearly seen that the MoS 2 The nanosheets retain their original ultra-thin structure. Further magnification reveals that ultra-fine clusters are loaded on the MoS 2 On the nanosheets, these ultrafine particles can be attributed to Ti 4 Cu 2 TiO nanoclusters after annealing x Cu y O z After calcination at 500℃, Ti x Cu y O z The average size of the clusters is basically the same as that before calcination, indicating that no agglomeration occurs during the calcination process.
[0141] Figure 3 The single component Ti-O, Ti obtained in Examples 1-4 of the present invention is presented. 4 Cu 2 O NCs, MoS 2 NSs and composite Ti-O NCs / MoS 2 NSs(MT-0),Ti 4 Cu 2 O NCs / MoS 2 The hydrogen evolution efficiency of NSs (MT-1, MT-5, MT-10) under (a) different sacrificial agents, (b) annealing or not, (c) the trend of hydrogen evolution efficiency and total hydrogen production (including MT-5A) after 12h of continuous reaction, and (d) the cycle test of sample MT-5A during 60h of reaction. The single component Ti-O nanoclusters, Ti 4 Cu 2 O nanoclusters, MoS 2 Nanosheets and composite nanomaterials Ti-O NCs / MoS 2 NSs(MT-0),Ti 4 Cu 2 O NCs / MoS 2 The photocatalytic activity of NSs (MT-1, MT-5, MT-10) was studied, and factors such as the type of sacrificial agent, calcination conditions and cycle stability were investigated.
[0142] like Figure 3 First, methanol and triethanolamine were used as sacrificial agents, and seven samples were added in sequence under the same light intensity (200 mW / cm -2 ) The hydrogen evolution efficiency after 1 h of reaction is as follows Figure 3 (a), it is obvious that when triethanolamine is used as a sacrificial agent, all seven samples have a higher hydrogen evolution efficiency, indicating that triethanolamine is more efficient as an electron donor in this system. Therefore, triethanolamine was used as a sacrificial agent in the subsequent performance tests of this series of catalysts. Secondly, the 1h hydrogen evolution efficiency of the seven samples with or without annealing conditions was investigated. Figure 3 (b) It is obvious that after calcination at 500℃, the Ti-O nanoclusters and Ti 4 Cu 2 The hydrogen evolution efficiencies of the O clusters and composite nanomaterials MT-0A, MT-1A, MT-5A, and MT-10A were improved to varying degrees. The improvement in activity may be attributed to two reasons: 1. The Ti 4 Cu 2 The organic ligands in the O nanoclusters expose more metal active sites; ② Calcination promotes the4 Cu 2 O clusters and MoS 2 The interfacial contact between them improves the charge transfer efficiency between them.
[0143] The 12h continuous hydrogen evolution reaction curves of 8 samples are as follows Figure 3 As shown in (c), the hydrogen evolution efficiency of the five composite materials is significantly improved compared with the three single-component materials, indicating that Ti 4 Cu 2 O nanoclusters were successfully loaded onto MoS 2 The nanosheets are bonded to form a heterojunction with them, providing more active sites for the composite material, significantly improving its photocatalytic hydrogen evolution efficiency and making up for the MoS 2 The nanosheets have few active sites, especially sample MT-5A, whose hydrogen evolution efficiency reached 5531.7 μmol·g -1 ·h -1 The total amount of hydrogen evolution in the first 12 hours reached 53764.4 μmol·g -1 .
[0144] Figure 4 The Ti obtained in the embodiment of the present invention is presented 4 Cu 2 O NCs, MoS 2 NSs、Ti 4 Cu 2 O / MoS 2 Nanocomposites (MT-5A) and Ti-O NCs / MoS 2 (a) Photoresponse current; (b) Electrochemical impedance spectroscopy; (c) Photoluminescence spectrum of NSs nanocomposite (MT-0A). 4 Cu 2 O NCs and MoS 2 NSs), respectively, with Ti 4 Cu 2 O NCs, MoS 2 NSs, MT-0A and MT-5A were used as active coatings on conductive glass (ITO) to make working electrodes, platinum mesh (Pt) and silver / silver chloride (Ag / AgCl) were used as counter electrode and reference electrode, respectively, and the photoresponse current was tested in a three-electrode system. Figure 4 As shown in (a), the working electrode coated with the MT-5A composite material has the largest photoresponse current density under visible light irradiation, and its magnitude is MT-0, Ti 4 Cu 2 O NCs and MoS 21.5, 4.4 and 7.6 times of that of NSs-coated electrodes, indicating that Ti in MT-5A composite nanomaterials 4 Cu 2 O NCs and MoS 2 A heterojunction is formed between NSs, which enhances the separation of photoinduced electrons and holes, while the presence of Cu also improves the photoresponse current density of the composite. Since the charge transfer rate is related to electrochemical impedance, electrochemical impedance spectroscopy (EIS) was performed on electrodes made from four different samples in this experiment.
[0145] like Figure 4 As shown in (b), in the high frequency range, the electrochemical impedance curves of the four materials are all semicircular, and their diameters are from large to small: MoS 2 NSs>Ti 4 Cu 2 O NCs>MT-0>MT-5A, indicating that Ti in MT-5A composite nanomaterials 4 Cu 2 O NCs and MoS 2 The heterojunction formed by NSs makes the contact between the two closer, the charge transfer resistance between them is the lowest, and the charge transfer efficiency is the highest, which is one of the reasons for the excellent photocatalytic activity. In addition, the presence of Cu has a positive significance for improving the conductivity of the composite material. Figure 4 As shown in (c), Ti 4 Cu 2 O NCs and MoS 2 The formation of heterojunctions between NSs is also affected by the MoS 2 The photoluminescence (PL) intensity decreases. At an excitation wavelength of λ = 250nm, the luminescence intensity of the composite material MT-5 is lower than that of Ti 4 Cu 2 O NCs, MoS 2 NSs and MT-0, further confirming that the MT-5A composite material has a significant photoinduced electron-hole pair separation rate.
[0146] Based on the above tests and analysis of photoresponse current density, electrochemical impedance and photoluminescence spectrum, it can be concluded that Ti 4 Cu 2 O NCs and MoS 2 The heterojunction formed between NSs can greatly improve the efficiency of photogenerated charge separation, accelerate the electron transfer rate, and is beneficial to the improvement of photocatalytic activity. Among them, Cu atoms play a positive role in improving the photoelectric performance of composite materials.
[0147] In summary, in Examples 1-4 of the present invention, a copper precursor is first synthesized by a simple method, and then a composite material Ti is synthesized by a one-step hydrothermal method and a coagulation precipitation method.4 Cu 2 O NCs / MoS 2 NSs, Ti-O NCs / MoS 2 NSs. Ti is decomposed by further calcination at high temperature. 4 Cu 2 Organic ligands in O nanoclusters and Ti-O nanoclusters can further improve the photocatalytic hydrogen evolution efficiency of the composite material. This provides a new way to design efficient photocatalysts for industrial applications and a new solution for the low-cost sustainable use of clean energy.
[0148] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.
Claims
1. A method for preparing a composite photocatalyst, characterized in that the steps include: Provide Ti x Cu y O z NCs; Providing MoS2 NSs; Loading MoS2 NSs onto Ti x Cu y O z NCs, Ti x Cu y O z Composite photocatalyst of clusters and MoS2 nanosheets; Among them, x and z are both positive numbers, and y is a number ≥0.
2. The preparation method according to claim 1, characterized in that: The Ti x Cu y O z The composite photocatalyst of clusters and MoS2 nanosheets was also calcined.
3. The preparation method according to claim 2, characterized in that: The calcination temperature is set according to its thermogravimetric curve. Specifically, the calcination temperature is the temperature at which the organic ligand is completely removed. Preferably, The calcination temperature is not lower than the "residual mass stabilization temperature" of the thermogravimetric curve.
4. The preparation method according to claim 1, characterized in that: The Ti x Cu y O z The preparation method of NCs comprises the following steps: providing a copper precursor; The copper precursor, benzoic acid, triethylamine and isopropyl titanate are mixed and reacted in a first solvent to obtain Ti x Cu y O z NCs.
5. The preparation method according to claim 4, characterized in that: The method for preparing the copper precursor comprises the following steps: Cu2O, tetrafluoroboric acid and a cyanide-containing compound are mixed and reacted to obtain [Cu(CH3CN)4]BF4, i.e., a copper precursor; preferably, After the reaction of Cu2O, tetrafluoroboric acid and the cyano-containing compound is completed, cooling and crystallization are performed to obtain a copper precursor; and / or The reaction temperature of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is 50-100° C., preferably 60-90° C., more preferably 70-80° C.; and / or The reaction time of the copper precursor, benzoic acid, triethylamine and isopropyl titanate is 12-72 hours, preferably 24-60 hours, and more preferably 36-48 hours.
6. The preparation method according to claim 1, characterized in that: The preparation method of the MoS2 NSs comprises the following steps: Mixing ammonium molybdate and a sulfur source in a second solvent and reacting them to obtain MoS2NSs; and / or The reaction temperature of the ammonium molybdate and the sulfur source is 180-300°C, preferably 210-240°C, more preferably 220-230°C; and / or The reaction time of the ammonium molybdate and the sulfur source is 5-24 hours, preferably 8-20 hours, and more preferably 10-18 hours.
7. The preparation method according to claim 1, characterized in that: The MoS2NSs are loaded onto Ti x Cu y O z NCs, the steps include: MoS2 NSs, Ti x Cu y O z NCs are mixed in a third solvent; preferably, MoS2 NSs、Ti x Cu y O z Before the NCs are mixed in the third solvent, MoS2 NSs are added to the third solvent and mixed to obtain a MoS2 NSs solution; Ti x Cu y O z NCs are added to the third solvent and mixed to obtain Ti x Cu y O z NCs solution; preferably, Ti x Cu y O z The NCs solution was added dropwise to the MoS2 NSs solution and mixed to obtain an intermediate product.
8. The preparation method according to claim 1, characterized in that: MoS2NSs loaded onto Ti x Cu y O z NCs, MoS2NSs, Ti x Cu y O z The material ratio of NCs is 1:(1-20), preferably 1:(1-15), and more preferably 1:(1-10).
9. A Ti x Cu y O z The composite photocatalyst of clusters and MoS2 nanosheets is characterized by: Obtained based on the preparation method according to any one of claims 1 to 8.
10. Ti according to claim 9 x Cu y O z The application of the composite photocatalyst of clusters and MoS2 nanosheets is characterized in that: The composite photocatalyst is applied to water electrolysis catalyst, especially to hydrogen evolution catalyst.