Method for selecting 38%-grade titanium middling from low-grade vanadium titano-magnetite
Through the steps of slag isolation treatment, concentration, weak magnetization iron removal and spiral reselection, the problem of low-grade vanadium titanium magnetite is solved, and the efficient selection of 38% grade titanium medium ore is achieved, reducing the number of spiral equipment. Improved production capacity and efficiency.
Patent Information
- Application Number
- CN202411324330.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
The existing ore dressing method has low efficiency in selecting titanium ore in low-grade vanadium titanium magnetite, and the large number of spiral equipment is wasted and the efficiency is not high.
Through slag isolation treatment, concentration, weak magnetic iron removal, spiral reselection and spiral hoist dehydration, the grade of titanium ore is gradually improved, thereby reducing the number of spirals and improving ore dressing efficiency.
It has achieved efficient selection of 38% grade titanium medium ore from low-grade vanadium titanium magnetite, reducing production costs and increasing the output and capacity of titanium medium ore.
Smart Images

Figure CN119056576A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ore dressing, and in particular to a method for selecting 38% grade titanium middlings from low grade vanadium-titanium magnetite. Background Art
[0002] The main types of ores in the Panxi area are vanadium-titanium magnetite, and the off-surface ore in the Baima mining area is mainly low-grade vanadium-titanium magnetite with a titanium grade of about 3.5%. The process for producing titanium middlings is mainly to grind, magnetically separate iron, and re-separate titanium from low-grade vanadium-titanium magnetite with a titanium grade of about 3.5%. The principle of titanium re-separation is to separate the differences in relative density, particle size, and shape between mineral particles and their movement speed and direction in the medium (water, air or other relatively dense liquids) to separate them from each other. The main solution for selecting titanium middlings in the Panxi area is spiral re-separation. Most concentrators often arrange a large number of spirals for titanium selection when the amount of titanium ore is not large. This method not only wastes floor space, but also has low efficiency in selecting titanium ore. Summary of the invention
[0003] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite, so as to solve the problem of low efficiency of selecting titanium ore in the existing beneficiation methods.
[0004] The technical solution of the present invention to solve the above technical problem is as follows: a method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite is provided, comprising the following steps:
[0005] (1) subjecting the titanium ore to slag separation to obtain coarse material and fine material;
[0006] (2) concentrating the fine material obtained in step (1);
[0007] (3) passing the concentrated ore in step (2) through two magnetic separators for magnetic separation and iron removal;
[0008] (4) subjecting the ore after iron removal in step (3) to spiral roughing to obtain gravity separation concentrate, middlings and tailings;
[0009] (5) subjecting the middlings from step (4) to spiral gravity separation to obtain gravity separation concentrate;
[0010] (6) scavenging the tailings from step (4) to obtain a gravity separation concentrate;
[0011] (7) The gravity separation concentrate obtained in steps (4) to (6) is subjected to four rounds of concentration to obtain.
[0012] Furthermore, the TiO2 content in low-grade vanadium-titanium magnetite is 3-5%.
[0013] Furthermore, in step (1), the particle size of the coarse material is greater than 1 mm, and the particle size of the fine material is not greater than 1 mm.
[0014] Furthermore, the concentration of the fine material after concentration in step (2) is 25-35 wt%.
[0015] Furthermore, in step (3), the magnetic field intensity of the magnetic separation for iron removal is 300-350 mT, and the feed concentration is 30-40 wt%.
[0016] Furthermore, the number of spirals in the spiral roughing process in step (4) is 45-48 groups.
[0017] Furthermore, the number of helices reselected in step (5) is 55-60 groups.
[0018] Furthermore, the number of spirals scanned and selected in step (6) is 55-60 groups.
[0019] Furthermore, the number of spirals selected in the four times in step (7) is 30-36 groups, 30-36 groups, 20-24 groups and 10-12 groups respectively.
[0020] The present invention has the following beneficial effects: the ore dressing method of the present invention obtains 38% grade titanium medium ore through slag separation, concentration, weak magnetic iron removal, spiral re-selection and spiral elevator dehydration. The ore dressing method of the present invention can reduce the number of spirals used in ore dressing, thereby reducing production costs, and can also obtain the maximum titanium medium ore output. The ore dressing method of the present invention can meet the maximum raw ore output of 240 tons / hour, and the output can reach 8-10 tons / hour. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the process flow of the mineral processing method of the present invention. DETAILED DESCRIPTION
[0022] The following examples are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0023] Example 1
[0024] A method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite, comprising the following steps:
[0025] (1) Using a linear screen to screen the 3.5% grade titanium ore to obtain coarse material and fine material, wherein the mesh size of the linear screen is 1 mm;
[0026] (2) concentrating the fine material obtained in step (1);
[0027] (3) The ore concentrated in step (2) is passed through two CTN1236 magnetic separators for iron removal;
[0028] (4) subjecting the ore after iron removal in step (3) to spiral roughing to obtain gravity separation concentrate, middlings and tailings, wherein the number of spiral roughing spirals is 48 groups;
[0029] (5) subjecting the middlings of step (4) to spiral gravity separation to obtain gravity separation concentrate, wherein the number of spirals for spiral gravity separation is 60 groups;
[0030] (6) subjecting the tailings of step (4) to scavenging to obtain gravity separation concentrate, wherein the number of scavenging spirals is 60 groups;
[0031] (7) The gravity separation concentrate obtained in steps (4) to (6) is subjected to four rounds of concentrating to obtain titanium middlings, wherein the number of spirals in the four rounds of concentrating is 36 groups, 36 groups, 24 groups and 12 groups respectively;
[0032] (8) Dehydrating the titanium ore obtained in step (7) using a screw elevator to obtain a 38% grade titanium ore.
[0033] Example 2
[0034] A method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite, comprising the following steps:
[0035] (1) Using a linear sieve to separate the 3% grade titanium ore to obtain coarse material and fine material, wherein the mesh size of the linear sieve is 1 mm;
[0036] (2) concentrating the fine material obtained in step (1);
[0037] (3) The ore concentrated in step (2) is passed through two CTN1236 magnetic separators for iron removal;
[0038] (4) subjecting the ore after iron removal in step (3) to spiral roughing to obtain gravity separation concentrate, middlings and tailings, wherein the number of spiral roughing spirals is 45 groups;
[0039] (5) subjecting the middlings of step (4) to spiral gravity separation to obtain gravity separation concentrate, wherein the number of spirals for spiral gravity separation is 55 groups;
[0040] (6) subjecting the tailings of step (4) to scavenging to obtain gravity separation concentrate, wherein the number of scavenging spirals is 55 groups;
[0041] (7) The gravity separation concentrate obtained in steps (4) to (6) is subjected to four rounds of concentrating to obtain titanium middlings, wherein the number of spirals in the four rounds of concentrating is 30 groups, 30 groups, 20 groups and 10 groups respectively;
[0042] (8) Dehydrating the titanium ore obtained in step (7) using a screw elevator to obtain a 38% grade titanium ore.
[0043] Example 3
[0044] A method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite, comprising the following steps:
[0045] (1) Using a linear sieve to separate 5% grade titanium ore to obtain coarse material and fine material, wherein the mesh size of the linear sieve is 1 mm;
[0046] (2) concentrating the fine material obtained in step (1);
[0047] (3) The ore concentrated in step (2) is passed through two CTN1236 magnetic separators for iron removal;
[0048] (4) subjecting the ore after iron removal in step (3) to spiral roughing to obtain gravity separation concentrate, middlings and tailings, wherein the number of spiral roughing spirals is 46 groups;
[0049] (5) subjecting the middlings of step (4) to spiral gravity separation to obtain gravity separation concentrate, wherein the number of spirals for spiral gravity separation is 58 groups;
[0050] (6) subjecting the tailings of step (4) to scavenging to obtain gravity separation concentrate, wherein the number of scavenging spirals is 58 groups;
[0051] (7) The gravity separation concentrate obtained in steps (4) to (6) is subjected to four rounds of concentrating to obtain titanium middlings, wherein the number of spirals in the four rounds of concentrating is 33 groups, 33 groups, 22 groups and 12 groups respectively;
[0052] (8) Dehydrating the titanium ore obtained in step (7) using a screw elevator to obtain a 38% grade titanium ore.
[0053] The technical parameters and operation technical indicators of the equipment involved in Examples 1-3 are as follows:
[0054] (1) Slag separation technical parameters are shown in Table 1.
[0055] Table 1 Technical parameters of slag separation equipment
[0056] Job Name Device Name model Screen Model <![CDATA[Sieving area (m 2 )]]> Number of units Slag separation Linear screen LKLB3673 300*610, mesh size 1mm*12mm 26.28 1
[0057] (2) Technical parameters of the concentration equipment are shown in Table 2.
[0058] Table 2 Technical parameters of concentration equipment
[0059] Job Name Device Name <![CDATA[Precipitation area (m 2 )]]> Concentration near mine (%) Underflow concentration (%) Overflow concentration (%) Number of units concentrate Concentration box 400 15 25-35 ≤3 1
[0060] (3) Technical indicators of weak magnetic iron removal operation are shown in Table 3.
[0061] Table 3 Technical indicators of weak magnetic iron removal operation
[0062]
[0063] (4) The technical parameters of the gravity separation equipment are shown in Table 4.
[0064] Table 4 Technical parameters of gravity separation equipment
[0065]
[0066] (5) Technical parameters of titanium dehydration equipment
[0067] Table 5 Dehydration technical parameters
[0068] Job Name Device Name Feed concentration (%) Ore concentration (%) Processing capacity (t / h) Quantity (unit) Dehydration Screw elevator 30-40 ≥80 >10 1
[0069] Comparative Example
[0070] The titanium production process of a certain ore dressing plant in Panxi area is that the tailings after iron selection are directly put into the spiral equipment for titanium selection without concentration. The number of spirals used in its production is more than 400 groups, and the production process is respectively roughing, middling reselection, fine first, fine second, fine third, and scavenging. Its production capacity is 4-6 tons / hour. However, by adopting the ore dressing method of the present invention, the number of spirals used in its production is more than 200 groups, and the production capacity can reach 8-10 tons / hour. It can be seen that the use of the invention method of the present application can reduce the number of spirals, reduce production costs, and improve production capacity at the same time.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for selecting 38% grade titanium middlings from low-grade vanadium-titanium magnetite, characterized in that: The following steps are involved: (1) subjecting the titanium ore to slag separation to obtain coarse material and fine material; (2) concentrating the fine material obtained in step (1); (3) The ore concentrated in step (2) is subjected to magnetic separation and iron removal by a magnetic separator; (4) roughing the ore after iron removal in step (3) to obtain re-selected concentrate, middlings and tailings; (5) subjecting the middlings from step (4) to spiral gravity separation to obtain gravity separation concentrate; (6) scavenging the tailings from step (4) to obtain a gravity separation concentrate; (7) The gravity separation concentrate obtained in steps (4) to (6) is subjected to four rounds of concentration to obtain.
2. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The TiO2 content in the low-grade vanadium-titanium magnetite is 3-5wt%.
3. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: In step (1), the particle size of the coarse material is greater than 1 mm, and the particle size of the fine material is not greater than 1 mm.
4. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The concentration of the fine material after concentration in step (2) is 25-35wt%.
5. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The magnetic field intensity of the magnetic separation and iron removal in step (3) is 300-350mT, and the feed concentration is 30-40wt%.
6. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The rough selection in step (4) adopts the spiral reselection method, wherein the number of spirals is 45-48 groups.
7. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The number of spirals reselected in step (5) is 55-60 groups.
8. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The scanning in step (6) adopts a spiral reselection method, wherein the number of spirals is 55-60 groups.
9. The method for extracting 38% grade titanium middlings from low-grade vanadium-titanium magnetite according to claim 1, characterized in that: The four rounds of selection in step (7) are all performed by spiral reselection, wherein the number of spirals is 30-36 groups, 30-36 groups, 20-24 groups and 10-12 groups respectively.