Secondary treatment process for slag recovery
By crushing, magnetic separation, acid leaching and resource processing of blast furnace slag, composite adsorbent with adsorption and photocatalytic degradation capabilities, as well as composite phase change heat storage materials with high temperature thermal stability, the utilization rate of blast furnace slag is solved. The problem of low and titanium-containing blast furnace slag recycling is difficult, which improves resource utilization efficiency and performance of finished products.
Patent Information
- Application Number
- CN202411111988.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing technology has a single form of blast furnace slag, low utilization rate, and cannot effectively exert its component characteristics. The recycling and use ratio of titanium-containing blast furnace slag is low, and the resource utilization is difficult, which limits its wide application.
A slag recovery secondary treatment process is adopted, including crushing, ball milling, screening, magnetic separation, acid leaching, washing, drying and grinding of titanium-containing blast furnace slag, and the titanium-silicon composite matrix material and composite adsorbent are prepared, and the The reaction of β-cyclodextrin forms a composite adsorbent, which is then subjected to resource-based secondary treatment and preparation of composite phase change heat storage materials, and is molded using inorganic salt phase change materials and binders.
It realizes efficient recycling and utilization of titanium and silicon components, prepares composite adsorbents with good adsorption properties and photocatalytic degradation capabilities, and composite phase change heat storage materials with high temperature thermal stability and chemical stability, and improves the titanium-containing blast furnace slag Resource utilization efficiency reduces production costs.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of slag resource treatment, and more specifically, to a slag recovery secondary treatment process. Background Art
[0002] Blast furnace slag is a byproduct of blast furnace smelting, which is formed by the gangue in the ore, the ash in the fuel and the non-volatile components in the flux. It is a solid waste generated in the metallurgical industry production process. Because it contains rich iron, calcium, silicon, titanium and magnesium, it has potential recycling value. If it is not effectively utilized and treated, blast furnace slag will pollute the environment and waste a lot of resources.
[0003] By making comprehensive use of blast furnace slag, the goal of converting waste into valuable resources can be achieved. At present, the treatment and utilization of blast furnace slag in my country is mainly to produce cement, building materials, road base materials, etc. with blast furnace slag as raw materials. These utilizations are mainly simple physical applications, with shortcomings such as single utilization form, low utilization rate, and low efficiency. They cannot effectively play the characteristics of each component in blast furnace slag, and cannot achieve the social and economic benefits that blast furnace slag should have. In addition, the current slag treatment technology is not perfect enough, and there is still a lack of comprehensive, applicable and cost-effective slag treatment technology. For example, the utilization methods of titanium-containing blast furnace slag are relatively limited, and there are problems such as low recycling ratio, high difficulty in resource utilization, and low efficiency, which limits the widespread application of the comprehensive utilization of titanium-containing blast furnace slag. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a slag recovery secondary treatment process.
[0005] A slag recovery secondary treatment process comprises the following steps:
[0006] S1: Recovery and processing of titanium-containing blast furnace slag, including crushing, ball milling, screening and magnetic separation of titanium-containing blast furnace slag;
[0007] S2: Resource treatment of titanium-containing blast furnace slag, adding the titanium-containing blast furnace slag after magnetic separation into a nitric acid solution, heating in a water bath, stirring the reaction, and filtering to obtain leached slag and filtrate, washing, drying, cooling and grinding the leached slag to obtain a titanium-silicon composite matrix material, and collecting the filtrate for later use;
[0008] S3: Preparation of composite adsorbent, stirring the β-cyclodextrin aqueous solution and the titanium-silicon composite matrix material to react, then adding a cross-linking agent, and continuously stirring until the liquid is in a solidified state to obtain a solidified body, which is then dried and ground to obtain a composite adsorbent;
[0009] S4: secondary resource recovery treatment, stirring the filtrate collected in step S2 with a sodium carbonate solution, filtering to obtain a precipitate A and a reaction mixed filtrate, adding a sodium hydroxide solution to the reaction mixed filtrate, stirring to react, filtering to obtain a precipitate B, mixing the precipitate A with the precipitate B, heating at a high temperature in an air atmosphere, and grinding to obtain a mixture powder;
[0010] S5: Preparation of composite phase change heat storage material: the mixture powder, inorganic salt phase change material and binder are mixed and ball-milled, and then molded, pressed, demolded, heated at high temperature and kept warm to obtain the composite phase change heat storage material.
[0011] Further, step S2: resource treatment of titanium-containing blast furnace slag specifically includes the following steps:
[0012] S2.1: Add the titanium-containing blast furnace slag after magnetic separation to a nitric acid solution with a mass fraction of 12-15%, wherein the solid-liquid weight ratio of the titanium-containing blast furnace slag after magnetic separation to the nitric acid solution is 1:(6-10), stir evenly, place in a constant temperature water bath at 70-80°C, and stir to react for 1-2h;
[0013] S2.2: After the reaction is completed, the leaching residue and the filtrate are obtained by suction filtration, and the leaching residue is washed 2 to 5 times with deionized water, and the filtrate is collected for later use;
[0014] S2.3: Subsequently, the washed leached residue is placed in an oven at 60-80° C. and dried for 8-10 hours, and then cooled and ground to obtain a titanium-silicon composite matrix material.
[0015] Further, step S3: preparing the composite adsorbent, specifically comprises the following steps:
[0016] S3.1: Add β-cyclodextrin into deionized water and stir to mix, the solid-liquid weight ratio is 1:(80-100), stir at 40-65°C for 20-40 minutes, until β-cyclodextrin is completely dissolved, to obtain a β-cyclodextrin aqueous solution;
[0017] S3.2: adding a titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution, wherein the solid-liquid weight ratio of the titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution is 1:(70-90), stirring the reaction at 35-50° C. for 1-2 hours, then adding a crosslinking agent, and continuously stirring until the liquid is solidified to obtain a solidified body;
[0018] S3.3: Place the solidified body in an oven at 70-80°C to dry, and grind it to obtain a composite adsorbent.
[0019] Furthermore, the amount of the cross-linking agent used is 3-7% of the total mass of the titanium-silicon composite matrix material and the β-cyclodextrin aqueous solution.
[0020] Furthermore, the cross-linking agent is a 25% by mass glutaraldehyde aqueous solution.
[0021] Further, step S4: secondary processing of resources, specifically including the following steps:
[0022] S4.1: Pour the collected filtrate into a reactor, and add a 10% sodium carbonate solution by mass into the reactor, the weight ratio of the filtrate to the sodium carbonate solution is 1:(1-2), stir and react for 20-30 minutes, filter, and obtain a precipitate A and a reaction mixed filtrate;
[0023] S4.2: Add 15% sodium hydroxide solution by mass to the reaction mixture filtrate, the weight ratio of the reaction mixture filtrate to the sodium hydroxide solution is 1:(0.4-1), stir the reaction for 20-30 minutes, filter, and obtain precipitate B;
[0024] S4.3: mixing precipitate A with precipitate B to obtain a precipitate mixture;
[0025] S4.4: Place the precipitated mixture in a ceramic crucible, then place the ceramic crucible in a muffle furnace, heat from room temperature to 500-540°C at a heating rate of 2-5°C / min in an air atmosphere, then keep warm for 30-60 minutes, and grind to obtain a mixture powder.
[0026] Further, step S5: preparing the composite phase change heat storage material, specifically comprises the following steps:
[0027] S5.1: adding the mixture powder, the inorganic salt phase change material and the binder into a planetary ball mill, mixing and ball milling at a speed of 200 to 400 r / min for 20 to 30 min, wherein the weight ratio of the mixture powder to the inorganic salt phase change material is (1 to 2): (1 to 3), to obtain a mixed powder;
[0028] S5.2: Put the mixed powder into a cylindrical mold, apply a pressure of 30 to 54 MPa to the mold on a press and maintain the pressure for 2 to 3 minutes, demold, and obtain a cylindrical composite material blank with a diameter of 10 to 18 mm and a thickness of 2 to 4 mm;
[0029] S5.3: Place the cylindrical composite material blank in a ceramic crucible, then place the ceramic crucible in a muffle furnace, and heat from room temperature to 90-120°C at a heating rate of 2-5°C / min in an air atmosphere, and maintain for 40-60 minutes to remove residual moisture. Then set the muffle furnace to continue heating to 340-360°C at a heating rate of 2-5°C / min, and then keep warm for 1-2 hours to obtain a composite phase change heat storage material. Subsequently, take out the composite phase change heat storage material and naturally cool it to room temperature, and store it in a drying oven for later use.
[0030] Furthermore, the inorganic salt phase change material is at least one of lithium carbonate, sodium nitrate, potassium nitrate, magnesium chloride, lithium fluoride, potassium fluoride, and potassium carbonate.
[0031] Furthermore, the amount of the binder used is 2-5% of the total mass of the mixture powder and the inorganic salt phase change material.
[0032] Furthermore, the binder is at least one of a mixture of polyvinyl alcohol aqueous solution and borax, bentonite, and sodium humate-modified bentonite.
[0033] The present invention has the following advantages:
[0034] 1. In the present invention, after the titanium-containing blast furnace slag is treated with acid leaching, the titanium-silicon composite matrix material mainly contains SiO2 and TiO2. The surface of the titanium-silicon composite matrix material contains a large number of hydroxyl groups, which is conducive to the combination of the titanium-silicon composite matrix material and β-cyclodextrin to form a composite adsorbent, and promotes the recycling and resource utilization of titanium and silicon components in the titanium-containing blast furnace slag: the hydroxyl groups on the surface of β-cyclodextrin and the hydroxyl groups on the surface of SiO2 in the titanium-silicon composite matrix material undergo dehydration condensation, and at the same time, hydrogen bonds are formed between TiO2 in the titanium-silicon composite matrix material and β-cyclodextrin, so that β-cyclodextrin is intercalated in the titanium-silicon composite matrix material. The obtained composite adsorbent has good adsorption properties and has a good adsorption effect on pollutants. At the same time, the titanium dioxide in the composite adsorbent undergoes a photocatalytic reaction to degrade the pollutants adsorbed on the surface of the material, maintains the efficient adsorption capacity and degradation performance of the composite adsorbent, and promotes the continuous adsorption.
[0035] 2. In the present invention, after resource recovery treatment, the collected filtrate contains soluble salts such as calcium, magnesium, aluminum and manganese. The filtrate is subjected to secondary resource recovery treatment, and the obtained mixture powder has calcium carbonate, magnesium oxide, aluminum oxide and manganese oxide as main components. The mixture powder has good thermal stability and chemical stability. The mixture powder is used as a substrate or filler in high temperature environment, which can ensure that the mixture powder still maintains its structure and performance stability in high temperature environment, plays an important role in the storage and utilization of renewable energy, improves the recycling and utilization effect of titanium-containing blast furnace slag, and improves the resource utilization efficiency of titanium-containing blast furnace slag.
[0036] 3. In the present invention, the mixed powder is used as the matrix material of the inorganic salt phase change material to prepare the composite phase change heat storage material. The prepared composite phase change heat storage material has good high-temperature thermal stability and thermal cycle stability, which not only reduces the production cost of the composite phase change heat storage material, but also realizes the value-added utilization of titanium-containing blast furnace slag, promotes the recycling and resource use of components such as calcium, magnesium and aluminum in the titanium-containing blast furnace slag, and reduces the harm of titanium-containing blast furnace slag to the environment. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] A slag recovery secondary treatment process specifically comprises the following steps:
[0040] S1: Recovery and processing of titanium-containing blast furnace slag
[0041] S1.1: crush, ball-mill and sieve the titanium-containing blast furnace slag to a particle size of 150 mesh;
[0042] S1.2: The screened titanium-containing blast furnace slag is sent to a magnetic separator for magnetic separation to remove strong magnetic substances, such as slag containing magnetic iron and elemental iron. The magnetic field strength of the magnetic separator is 1000GS;
[0043] S2: Resource treatment of titanium-containing blast furnace slag
[0044] S2.1: Add the titanium-containing blast furnace slag after magnetic separation into a nitric acid solution with a mass fraction of 15%, and the solid-liquid weight ratio of the titanium-containing blast furnace slag after magnetic separation to the nitric acid solution is 1:10. After stirring evenly, put it into a constant temperature water bath at 80°C and stir for 2 hours;
[0045] S2.2: After the reaction is completed, the leached residue and the filtrate are obtained by suction filtration. The leached residue is washed 5 times with deionized water, and the filtrate is collected for later use;
[0046] S2.3: Subsequently, the washed leached residue is placed in an oven at 80° C. and dried for 10 h, and then cooled and ground to obtain a titanium-silicon composite matrix material;
[0047] S3: Composite adsorbent preparation
[0048] S3.1: Add β-cyclodextrin into deionized water and stir to mix, the solid-liquid weight ratio is 1:100, stir at 65°C for 40 minutes, and wait until β-cyclodextrin is completely dissolved to obtain a β-cyclodextrin aqueous solution;
[0049] S3.2: Add a titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution, wherein the solid-liquid weight ratio of the titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution is 1:90, and stir the reaction at 50°C for 2 hours. Subsequently, add a 25% by mass glutaraldehyde aqueous solution, wherein the amount of the glutaraldehyde aqueous solution added is 5% of the total mass of the titanium-silicon composite matrix material and the β-cyclodextrin aqueous solution, and continue stirring until the liquid is solidified to obtain a solidified body;
[0050] S3.3: drying the solidified solid in an oven at 80°C, and grinding the solidified solid to obtain a composite adsorbent;
[0051] S4: Secondary processing of resources
[0052] S4.1: Pour the filtrate collected in step S2.2 into a reactor, and add a 10% sodium carbonate solution by mass into the reactor, the weight ratio of the filtrate to the sodium carbonate solution is 1:2, stir and react for 30 minutes, filter, and obtain a precipitate A and a reaction mixed filtrate;
[0053] S4.2: Add 15% sodium hydroxide solution by mass to the reaction mixture filtrate, the weight ratio of the reaction mixture filtrate to the sodium hydroxide solution is 1:1, stir and react for 30 minutes, filter and obtain precipitate B;
[0054] S4.3: mixing precipitate A with precipitate B to obtain a precipitate mixture;
[0055] S4.4: placing the precipitated mixture in a ceramic crucible, placing the ceramic crucible in a muffle furnace, heating from room temperature to 540°C at a heating rate of 5°C / min in an air atmosphere, then keeping the temperature for 60 minutes, and grinding to obtain a mixture powder;
[0056] S5: Preparation of composite phase change thermal storage materials
[0057] S5.1: Add the mixture powder, sodium nitrate and sodium humate modified bentonite into a planetary ball mill, and mix and ball-mill at a speed of 400 r / min for 30 min, wherein the weight ratio of the mixture powder to sodium nitrate is 2:3, and the amount of sodium humate modified bentonite is 5% of the total mass of the mixture powder and sodium nitrate, to obtain a mixed powder;
[0058] S5.2: Put the mixed powder into a cylindrical mold, apply a pressure of 54 MPa to the mold on a press and maintain the pressure for 3 minutes, demould, and obtain a cylindrical composite blank with a diameter of 10 mm and a thickness of 4 mm;
[0059] S5.3: Place the cylindrical composite material blank in a ceramic crucible, then place the ceramic crucible in a muffle furnace, and heat from room temperature to 120°C at a heating rate of 5°C / min in an air atmosphere, and keep it for 60 minutes to remove residual moisture. Then set the muffle furnace to continue heating to 360°C at a heating rate of 5°C / min, and then keep it warm for 2 hours to obtain a composite phase change heat storage material. Subsequently, take out the composite phase change heat storage material and naturally cool it to room temperature, and store it in a drying oven for later use.
[0060] Example 2
[0061] A slag recovery secondary treatment process specifically comprises the following steps:
[0062] S1: Recovery and processing of titanium-containing blast furnace slag
[0063] S1.1: crush, ball-mill and sieve the titanium-containing blast furnace slag to a particle size of 150 mesh;
[0064] S1.2: The screened titanium-containing blast furnace slag is sent to a magnetic separator for magnetic separation to remove strong magnetic substances, such as slag containing magnetic iron and elemental iron. The magnetic field strength of the magnetic separator is 1000GS;
[0065] S2: Resource treatment of titanium-containing blast furnace slag
[0066] S2.1: Add the titanium-containing blast furnace slag after magnetic separation into a nitric acid solution with a mass fraction of 15%, and the solid-liquid weight ratio of the titanium-containing blast furnace slag after magnetic separation to the nitric acid solution is 1:10. After stirring evenly, put it into a constant temperature water bath at 70°C and stir for 1 hour;
[0067] S2.2: After the reaction is completed, the leached residue and the filtrate are obtained by suction filtration. The leached residue is washed twice with deionized water, and the filtrate is collected for later use;
[0068] S2.3: Subsequently, the washed leached residue is placed in an oven at 60° C. and dried for 8 h, and then cooled and ground to obtain a titanium-silicon composite matrix material;
[0069] S3: Composite adsorbent preparation
[0070] S3.1: Add β-cyclodextrin into deionized water and stir to mix, the solid-liquid weight ratio is 1:100, stir at 40°C for 20 minutes, and wait until β-cyclodextrin is completely dissolved to obtain a β-cyclodextrin aqueous solution;
[0071] S3.2: Add a titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution, wherein the solid-liquid weight ratio of the titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution is 1:90, and stir the reaction at 35°C for 1 hour. Subsequently, add a 25% by mass aqueous solution of glutaraldehyde, wherein the amount of the glutaraldehyde aqueous solution added is 5% of the total mass of the titanium-silicon composite matrix material and the β-cyclodextrin aqueous solution, and continue stirring until the liquid is solidified to obtain a solidified body;
[0072] S3.3: drying the solidified solid in an oven at 70°C, and grinding the solidified solid to obtain a composite adsorbent;
[0073] S4: Secondary processing of resources
[0074] S4.1: Pour the filtrate collected in step S2.2 into a reactor, and add a 10% sodium carbonate solution by mass into the reactor, the weight ratio of the filtrate to the sodium carbonate solution being 1:2, stir and react for 20 minutes, filter, and obtain a precipitate A and a reaction mixed filtrate;
[0075] S4.2: Add 15% sodium hydroxide solution by mass to the reaction mixture filtrate, the weight ratio of the reaction mixture filtrate to the sodium hydroxide solution is 1:1, stir and react for 20 minutes, filter and obtain precipitate B;
[0076] S4.3: mixing precipitate A with precipitate B to obtain a precipitate mixture;
[0077] S4.4: placing the precipitated mixture in a ceramic crucible, placing the ceramic crucible in a muffle furnace, heating from room temperature to 500°C at a heating rate of 2°C / min in an air atmosphere, and then keeping the temperature for 30 minutes, and grinding to obtain a mixture powder;
[0078] S5: Preparation of composite phase change thermal storage materials
[0079] S5.1: Add the mixture powder, sodium nitrate and sodium humate modified bentonite into a planetary ball mill, and mix and ball-mill at a speed of 200 r / min for 20 min, wherein the weight ratio of the mixture powder to sodium nitrate is 2:3, and the amount of sodium humate modified bentonite is 5% of the total mass of the mixture powder and sodium nitrate, to obtain a mixed powder;
[0080] S5.2: Put the mixed powder into a cylindrical mold, apply a pressure of 30 MPa to the mold on a press and maintain the pressure for 2 minutes, demould, and obtain a cylindrical composite blank with a diameter of 10 mm and a thickness of 4 mm;
[0081] S5.3: Place the cylindrical composite material blank in a ceramic crucible, then place the ceramic crucible in a muffle furnace, and heat from room temperature to 90°C at a heating rate of 2°C / min in an air atmosphere, and keep it for 40 minutes to remove residual moisture. Then set the muffle furnace to continue to heat up to 340°C at a heating rate of 2°C / min, and then keep it warm for 1 hour to obtain a composite phase change heat storage material. Subsequently, take out the composite phase change heat storage material and naturally cool it to room temperature, and store it in a drying oven for later use.
[0082] Example 3
[0083] A slag recovery secondary treatment process specifically comprises the following steps:
[0084] S1: Recovery and processing of titanium-containing blast furnace slag
[0085] S1.1: crush, ball-mill and sieve the titanium-containing blast furnace slag to a particle size of 180 mesh;
[0086] S1.2: The screened titanium-containing blast furnace slag is sent to a magnetic separator for magnetic separation to remove strong magnetic substances, such as slag containing magnetic iron and elemental iron. The magnetic field strength of the magnetic separator is 2000GS;
[0087] S2: Resource treatment of titanium-containing blast furnace slag
[0088] S2.1: Add the titanium-containing blast furnace slag after magnetic separation into a nitric acid solution with a mass fraction of 15%, and the solid-liquid weight ratio of the titanium-containing blast furnace slag after magnetic separation to the nitric acid solution is 1:6. After stirring evenly, put it into a constant temperature water bath at 80°C and stir for 2 hours;
[0089] S2.2: After the reaction is completed, the leached residue and the filtrate are obtained by suction filtration. The leached residue is washed 5 times with deionized water, and the filtrate is collected for later use;
[0090] S2.3: Subsequently, the washed leached residue is placed in an oven at 80° C. and dried for 10 h, and then cooled and ground to obtain a titanium-silicon composite matrix material;
[0091] S3: Composite adsorbent preparation
[0092] S3.1: Add β-cyclodextrin into deionized water and stir to mix, the solid-liquid weight ratio is 1:80, stir at 65°C for 40 minutes, until β-cyclodextrin is completely dissolved, to obtain a β-cyclodextrin aqueous solution;
[0093] S3.2: Add a titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution, wherein the solid-liquid weight ratio of the titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution is 1:70, and stir the reaction at 50°C for 2 hours. Subsequently, add a 25% by mass glutaraldehyde aqueous solution, wherein the amount of the glutaraldehyde aqueous solution added is 3% of the total mass of the titanium-silicon composite matrix material and the β-cyclodextrin aqueous solution, and continue stirring until the liquid is solidified to obtain a solidified body;
[0094] S3.3: drying the solidified solid in an oven at 80°C, and grinding the solidified solid to obtain a composite adsorbent;
[0095] S4: Secondary processing of resources
[0096] S4.1: Pour the filtrate collected in step S2.2 into a reactor, and add a 10% sodium carbonate solution by mass into the reactor, the weight ratio of the filtrate to the sodium carbonate solution being 1:1, stir and react for 30 minutes, filter, and obtain a precipitate A and a reaction mixed filtrate;
[0097] S4.2: Add 15% sodium hydroxide solution by mass to the reaction mixture filtrate, the weight ratio of the reaction mixture filtrate to the sodium hydroxide solution is 1:0.5, stir and react for 30 minutes, filter and obtain precipitate B;
[0098] S4.3: mixing precipitate A with precipitate B to obtain a precipitate mixture;
[0099] S4.4: placing the precipitated mixture in a ceramic crucible, placing the ceramic crucible in a muffle furnace, heating from room temperature to 540°C at a heating rate of 5°C / min in an air atmosphere, then keeping the temperature for 60 minutes, and grinding to obtain a mixture powder;
[0100] S5: Preparation of composite phase change thermal storage materials
[0101] S5.1: Add the mixture powder, sodium nitrate and sodium humate modified bentonite into a planetary ball mill, and mix and ball-mill at a speed of 400 r / min for 30 min, wherein the weight ratio of the mixture powder to sodium nitrate is 1:1, and the amount of sodium humate modified bentonite is 2% of the total mass of the mixture powder and sodium nitrate, to obtain a mixed powder;
[0102] S5.2: Put the mixed powder into a cylindrical mold, apply a pressure of 54 MPa to the mold on a press and maintain the pressure for 3 minutes, demould, and obtain a cylindrical composite blank with a diameter of 10 mm and a thickness of 4 mm;
[0103] S5.3: Place the cylindrical composite material blank in a ceramic crucible, then place the ceramic crucible in a muffle furnace, and heat from room temperature to 120°C at a heating rate of 5°C / min in an air atmosphere, and keep it for 60 minutes to remove residual moisture. Then set the muffle furnace to continue heating to 360°C at a heating rate of 5°C / min, and then keep it warm for 2 hours to obtain a composite phase change heat storage material. Subsequently, take out the composite phase change heat storage material and naturally cool it to room temperature, and store it in a drying oven for later use.
[0104] Comparative Example 1
[0105] Compared with Example 1, the difference of Comparative Example 1 is that the titanium-containing blast furnace slag after magnetic separation is directly used in the preparation of the composite adsorbent, the titanium-silicon composite matrix material in step S3.2 is replaced by the titanium-containing blast furnace slag after magnetic separation, and the other steps remain unchanged to prepare the composite adsorbent, which is recorded as Comparative Example 1.
[0106] 60 mg of the composite adsorbent obtained from Examples 1-3 and Comparative Example 1 were weighed as test samples, and each group of samples was dispersed in 100 mL of a methylene blue solution with a concentration of 0.01 g / L. The mixture was magnetically stirred for 60 min in the dark to obtain a mixed liquid. The mixed liquid was then irradiated under a 250 W high-pressure mercury lamp, reacted for 30 min, and 10 mL of the mixed liquid was taken out and centrifuged. After centrifugal separation, the concentration of the methylene blue solution in the solution was analyzed by ultraviolet-visible diffuse reflectance spectroscopy, and the degradation rate of the sample to methylene blue was calculated. The results are shown in Table 1.
[0107] The degradation rate calculation formula is:
[0108] Among them, N0 and N1 are the concentrations of methylene blue before and after degradation, respectively.
[0109] Table 1:
[0110] Group Degradation rate (%) Example 1 68.77 Example 2 65.93 Example 3 62.68 Comparative Example 1 27.31
[0111] As can be seen from Table 1, in the process of photocatalytic degradation of methylene blue, the composite adsorbent prepared in Examples 1-3 has a significantly stronger ability to degrade methylene blue than Comparative Example 1, and can play a good adsorption and degradation role. It is shown that although the composite adsorbent prepared by directly using titanium-containing blast furnace slag after magnetic separation as a raw material can have a certain ability to degrade pollutants, the adsorption treatment effect achieved is significantly weaker than that of the composite adsorbent in Examples 1-3. By resource-processing the titanium-containing blast furnace slag, the titanium-silicon composite matrix material obtained is combined with β-cyclodextrin for adsorption and degradation of pollutants, which can play a good adsorption and degradation role on pollutants, which is beneficial to greatly improve the recovery rate of titanium dioxide and silicon dioxide in the recovery process of titanium-containing blast furnace slag.
[0112] Comparative Example 2
[0113] Compared with Example 1, the difference of Comparative Example 2 is that the titanium-containing blast furnace slag after magnetic separation is directly used in the preparation of the composite phase change heat storage material, the mixed powder in step S5.1 is replaced by the titanium-containing blast furnace slag after magnetic separation, and the other steps remain unchanged to prepare the composite phase change heat storage material, which is recorded as Comparative Example 2.
[0114] The performance of the composite phase change heat storage materials obtained in Examples 1-3 and Comparative Example 2 was tested, wherein the test condition of the thermal cycle was 600° C. The results are shown in Table 2.
[0115] Table 2:
[0116] Group Thermal conductivity (W / m*K) Latent heat of phase change (J / g) Status after 100 thermal cycles Example 1 2.4 72.53 No deformation, no cracks Example 2 2.3 70.24 No deformation, no cracks Example 3 2.1 69.82 No deformation, no cracks Comparative Example 2 1.3 52.17 Crack formation
[0117] As can be seen from Table 2, the thermal conductivity of the composite phase change heat storage materials prepared in Examples 1-3 is all greater than 2W / m*K, and the test results of the phase change latent heat and the thermal cycle test results are also better than those of Comparative Example 2, indicating that Comparative Example 2 directly uses the titanium-containing blast furnace slag after magnetic separation as a raw material to prepare the composite phase change heat storage material, and the high-temperature thermal stability and thermal cycle stability achieved are weaker than those of the composite phase change heat storage materials in Examples 1-3. Examples 1-3 perform secondary resource recovery treatment on the titanium-containing blast furnace slag to obtain a mixture powder with good thermal stability and chemical stability. Its use as a substrate for the composite phase change heat storage material is conducive to the preparation of a composite phase change heat storage material with good high-temperature thermal stability and thermal cycle stability, and greatly improves the recovery rate of components such as calcium, magnesium and aluminum in the titanium-containing blast furnace slag and the effect of resource recovery.
[0118] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all such improvements and changes should fall within the scope of protection of the appended claims of the present invention. Parts not described in detail in this specification belong to the prior art known to those skilled in the art.
Claims
1. A slag recovery secondary treatment process, It is characterized in that The steps include: S1: Recovery and processing of titanium-containing blast furnace slag, including crushing, ball milling, screening and magnetic separation of titanium-containing blast furnace slag; S2: Resource treatment of titanium-containing blast furnace slag, adding the titanium-containing blast furnace slag after magnetic separation into a nitric acid solution, heating in a water bath, stirring the reaction, and filtering to obtain leached slag and filtrate, washing, drying, cooling and grinding the leached slag to obtain a titanium-silicon composite matrix material, and collecting the filtrate for later use; S3: Preparation of composite adsorbent, stirring the β-cyclodextrin aqueous solution and the titanium-silicon composite matrix material to react, then adding a cross-linking agent, and continuously stirring until the liquid is in a solidified state to obtain a solidified body, which is then dried and ground to obtain a composite adsorbent; S4: secondary resource recovery treatment, stirring the filtrate collected in step S2 with a sodium carbonate solution, filtering to obtain a precipitate A and a reaction mixed filtrate, adding a sodium hydroxide solution to the reaction mixed filtrate, stirring to react, filtering to obtain a precipitate B, mixing the precipitate A with the precipitate B, heating at a high temperature in an air atmosphere, and grinding to obtain a mixture powder; S5: Preparation of composite phase change heat storage material: the mixture powder, inorganic salt phase change material and binder are mixed and ball-milled, and then molded, pressed, demolded, heated at high temperature and kept warm to obtain the composite phase change heat storage material.
2. A slag recovery secondary treatment process according to claim 1, It is characterized in that Step S2: Resource treatment of titanium-containing blast furnace slag, specifically comprising the following steps: S2.1: Add the titanium-containing blast furnace slag after magnetic separation to a nitric acid solution with a mass fraction of 12-15%, wherein the solid-liquid weight ratio of the titanium-containing blast furnace slag after magnetic separation to the nitric acid solution is 1:(6-10), stir evenly, place in a constant temperature water bath at 70-80°C, and stir to react for 1-2h; S2.2: After the reaction is completed, the leaching residue and the filtrate are obtained by suction filtration, and the leaching residue is washed 2 to 5 times with deionized water, and the filtrate is collected for later use; S2.3: Subsequently, the washed leached residue is placed in an oven at 60-80° C. and dried for 8-10 hours, and then cooled and ground to obtain a titanium-silicon composite matrix material.
3. A slag recovery secondary treatment process according to claim 1, It is characterized in that Step S3: Preparation of composite adsorbent, specifically comprising the following steps: S3.1: Add β-cyclodextrin into deionized water and stir to mix, the solid-liquid weight ratio is 1:(80-100), stir at 40-65°C for 20-40 minutes, until β-cyclodextrin is completely dissolved, to obtain a β-cyclodextrin aqueous solution; S3.2: adding a titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution, wherein the solid-liquid weight ratio of the titanium-silicon composite matrix material to the β-cyclodextrin aqueous solution is 1:(70-90), stirring the reaction at 35-50° C. for 1-2 hours, then adding a crosslinking agent, and continuously stirring until the liquid is solidified to obtain a solidified body; S3.3: Place the solidified body in an oven at 70-80°C to dry, and grind it to obtain a composite adsorbent.
4. A slag recovery secondary treatment process according to claim 3, It is characterized in that The amount of the cross-linking agent used is 3-7% of the total mass of the titanium-silicon composite matrix material and the beta-cyclodextrin aqueous solution.
5. A slag recovery secondary treatment process according to claim 3, It is characterized in that The cross-linking agent is a 25% by mass glutaraldehyde aqueous solution.
6. A slag recovery secondary treatment process according to claim 1, It is characterized in that Step S4: secondary processing of resources, specifically including the following steps: S4.1: Pour the collected filtrate into a reactor, and add a 10% sodium carbonate solution by mass into the reactor, the weight ratio of the filtrate to the sodium carbonate solution is 1:(1-2), stir and react for 20-30 minutes, filter, and obtain a precipitate A and a reaction mixed filtrate; S4.2: Add 15% sodium hydroxide solution by mass to the reaction mixture filtrate, the weight ratio of the reaction mixture filtrate to the sodium hydroxide solution is 1:(0.4-1), stir the reaction for 20-30 minutes, filter, and obtain precipitate B; S4.3: mixing precipitate A with precipitate B to obtain a precipitate mixture; S4.4: Place the precipitated mixture in a ceramic crucible, then place the ceramic crucible in a muffle furnace, heat from room temperature to 500-540°C at a heating rate of 2-5°C / min in an air atmosphere, then keep warm for 30-60 minutes, and grind to obtain a mixture powder.
7. A slag recovery secondary treatment process according to claim 1, It is characterized in that Step S5: Preparation of composite phase change heat storage material, specifically including the following steps: S5.1: adding the mixture powder, the inorganic salt phase change material and the binder into a planetary ball mill, mixing and ball milling at a speed of 200 to 400 r / min for 20 to 30 min, wherein the weight ratio of the mixture powder to the inorganic salt phase change material is (1 to 2): (1 to 3), to obtain a mixed powder; S5.2: Put the mixed powder into a cylindrical mold, apply a pressure of 30 to 54 MPa to the mold on a press and maintain the pressure for 2 to 3 minutes, demold, and obtain a cylindrical composite material blank with a diameter of 10 to 18 mm and a thickness of 2 to 4 mm; S5.3: Place the cylindrical composite material blank in a ceramic crucible, then place the ceramic crucible in a muffle furnace, and heat from room temperature to 90-120°C at a heating rate of 2-5°C / min in an air atmosphere, and maintain for 40-60 minutes to remove residual moisture. Then set the muffle furnace to continue heating to 340-360°C at a heating rate of 2-5°C / min, and then keep warm for 1-2 hours to obtain a composite phase change heat storage material. Subsequently, take out the composite phase change heat storage material and naturally cool it to room temperature, and store it in a drying oven for later use.
8. A slag recovery secondary treatment process according to claim 7, It is characterized in that The inorganic salt phase change material is at least one of lithium carbonate, sodium nitrate, potassium nitrate, magnesium chloride, lithium fluoride, potassium fluoride and potassium carbonate.
9. A slag recovery secondary treatment process according to claim 8, It is characterized in that The amount of the binder used is 2-5% of the total mass of the mixture powder and the inorganic salt phase change material.
10. A slag recovery secondary treatment process according to claim 9, It is characterized in that The binder is at least one of a mixture of polyvinyl alcohol aqueous solution and borax, bentonite, and sodium humate modified bentonite.
Citation Information
Patent Citations
Phase change heat storage material and preparation method thereof
CN107779175A
Method for extracting components of titanium, iron, aluminum and magnesium in high-titanium slag through staged roasting
CN109321759A
Modified high-temperature-resistant polypropylene material and preparation method thereof
CN111909482A
Method for preparing energy storage material from secondary aluminum ash
CN116120901A
Method for solid sealing of harmful metals by using fly ash-titanium-containing blast furnace slag based geopolymer
CN117181767A