Method for manufacturing titanium alloy / nickel-based superalloy bimetallic component through metal powder laser directional energy deposition

By introducing a Cr/V bimetal transition layer at the interface between titanium alloy and nickel-based high-temperature alloy, the brittle intermetallic compound problem during direct bonding is solved, and good interface combination and high temperature of the bimetallic structure of titanium alloy/nickel-based high-temperature alloy is achieved. Domain service capability.

CN119057082AActive Publication Date: 2024-12-03BEIJING INST OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411187573.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

When the titanium alloy and nickel-based high-temperature alloy are directly bonded, the interface is prone to form brittle intermetallic compounds, resulting in cracking failure of the components during laser-oriented energy deposition, making it difficult to achieve effective bonding.

Method used

The Cr/V bimetallic deposition layer is used as the connecting transition layer to avoid the formation of intermetallic compounds between Ni and Ti elements, and the titanium alloy/nickel-based high-temperature alloy bimetallic structure is prepared using conventional metal powder laser directional energy deposition technology.

Benefits of technology

The good interface combination of titanium alloy/nickel-based high-temperature alloy bimetal structure is achieved, which avoids cracking failure during component preparation, and can build high-performance components in wide temperature range service in complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057082A_ABST
    Figure CN119057082A_ABST
Patent Text Reader

Abstract

The invention provides a method for manufacturing a titanium alloy / nickel-based superalloy bimetallic component through metal powder laser directional energy deposition, and relates to the technical field of additive manufacturing. In order to realize effective combination of the titanium alloy and the nickel-based superalloy and improve the interface strength of the titanium alloy and the nickel-based superalloy, a Cr / V bimetallic deposition layer is used as a connection transition layer, and the titanium alloy / nickel-based superalloy bimetallic structural part with good interface combination is prepared by using conventional metal powder laser directional energy deposition equipment. On the basis, construction of a titanium alloy / nickel-based high-temperature alloy bimetallic structure in a wide-temperature-range service component of a complex structure can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of additive manufacturing, and in particular to a method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directional energy deposition of metal powder. Background Art

[0002] The service temperature span of key aircraft components in the aerospace field is large. For example, the service temperature of aircraft engine turbine disks is between 700 and 1500°C, and different parts have different requirements for material properties. Titanium alloys and nickel-based superalloys are two types of metal structural materials widely used in the current aerospace field. Among them, titanium alloys have low density and high specific strength, and are suitable for high-temperature environments of 400 to 600°C; nickel-based superalloys have good high-temperature strength, creep resistance and high-temperature oxidation resistance, and can serve in environments of 700 to 1000°C. Using metal additive manufacturing technology to construct a titanium alloy / nickel-based superalloy bimetallic structure in a wide temperature range service component with a complex structure can realize the aircraft structural design characteristics of "different parts, different materials, and different performances", which is of great significance for effective weight reduction and improving the thrust-to-weight ratio of aircraft.

[0003] Due to the differences between titanium alloy and nickel-based superalloy in terms of main components and crystal structure, when the two materials are directly joined using metal powder laser directed energy deposition technology, a large amount of brittle intermetallic compounds are often formed at the interface of the two materials. The brittle intermetallic compounds will cause cracking and failure during the component preparation process under the huge thermal stress brought by laser directed energy deposition. Therefore, achieving effective bonding of titanium alloy and nickel-based superalloy and improving their interface strength is a major challenge in manufacturing titanium alloy / nickel-based superalloy bimetallic structures. Summary of the invention

[0004] The purpose of the present invention is to provide a method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directional energy deposition of metal powder. By using the method of the present invention to join a titanium alloy and a nickel-based high-temperature alloy, no brittle intermetallic compound is generated at the connection interface, and a titanium alloy / nickel-based high-temperature alloy bimetallic component with good interface bonding can be prepared.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directional energy deposition of metal powder, comprising the following steps:

[0007] Depositing nickel-based high-temperature alloy powder on the substrate to form a nickel-based high-temperature alloy deposition layer;

[0008] Depositing Cr metal powder on the surface of the nickel-based high-temperature alloy deposition layer to form a Cr metal deposition layer;

[0009] Depositing V metal powder on the surface of the Cr metal deposition layer to form a V metal deposition layer;

[0010] Titanium alloy powder is deposited on the surface of the V metal deposition layer to form a titanium alloy deposition layer, thereby obtaining a titanium alloy / nickel-based high-temperature alloy bimetallic component.

[0011] Preferably, the total thickness of the Cr metal deposition layer is 0.2-1 mm.

[0012] Preferably, the total thickness of the V metal deposition layer is 0.2-1 mm.

[0013] Preferably, the conditions for depositing the Cr metal powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

[0014] Preferably, the conditions for depositing the V metal powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

[0015] Preferably, the conditions for depositing the nickel-based high-temperature alloy powder include: substrate temperature of 200-1000° C., laser spot diameter of 0.5-3 mm, laser power of 350-2600 W, laser scanning rate of 300-1200 mm / min, and single-layer deposition thickness of 0.2-0.5 mm.

[0016] Preferably, the total thickness of the nickel-based high-temperature alloy deposition layer is 5 to 50 mm.

[0017] Preferably, the conditions for depositing the titanium alloy powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

[0018] Preferably, the total thickness of the titanium alloy deposited layer is 5 to 50 mm.

[0019] Preferably, the particle sizes of the nickel-based high-temperature alloy powder, the Cr metal powder, the V metal powder and the titanium alloy powder are independently 53 to 150 μm.

[0020] The present invention provides a method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directional energy deposition of metal powder, comprising the following steps: depositing nickel-based high-temperature alloy powder on a substrate to form a nickel-based high-temperature alloy deposition layer; depositing Cr metal powder on the surface of the nickel-based high-temperature alloy deposition layer to form a Cr metal deposition layer; depositing V metal powder on the surface of the Cr metal deposition layer to form a V metal deposition layer; depositing titanium alloy powder on the surface of the V metal deposition layer to form a titanium alloy deposition layer, thereby obtaining a titanium alloy / nickel-based high-temperature alloy bimetallic component.

[0021] Since the main element in nickel-based alloys is Ni and the main element in titanium alloys is Ti, the direct combination of titanium alloys and nickel-based high-temperature alloys will form a large amount of Ti-Ni intermetallic compounds at the interface, which can easily cause cracking and failure during the component preparation process. The present invention uses a Cr / V bimetallic deposition layer as a connecting transition layer. No intermetallic compounds are formed between the Ni element and the Cr element, no intermetallic compounds are formed between the Ti element and the V element, and no intermetallic compounds are formed between the Cr element and the V element. Therefore, the Cr / V bimetallic intermediate layer is used as a transition to construct a "nickel-based high-temperature alloy / Cr / V / titanium alloy" structure, which can effectively avoid the generation of intermetallic compounds at the interface and achieve a good interface bonding effect.

[0022] The present invention uses a reasonable intermediate layer design and conventional metal powder laser directed energy deposition equipment to prepare a titanium alloy / nickel-based high-temperature alloy bimetallic structure with good interface bonding. On this basis, the construction of a titanium alloy / nickel-based high-temperature alloy bimetallic structure in a wide temperature range service component with a complex structure can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The following are photos of the titanium alloy / nickel-based high-temperature alloy bimetallic samples prepared in Examples 1 to 3; wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3;

[0024] Figure 2 This is a microstructure morphology of the internal interface of the titanium alloy / nickel-based high-temperature alloy bimetallic sample prepared in Example 1;

[0025] Figure 3 This is an XRD characterization result diagram of the internal interface of the titanium alloy / nickel-based high-temperature alloy bimetallic sample prepared in Example 1;

[0026] Figure 4 This is the microstructure morphology and XRD characterization results of the internal interface of the direct bonding sample in comparative example 1. DETAILED DESCRIPTION

[0027] The present invention provides a method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directional energy deposition of metal powder, comprising the following steps:

[0028] Depositing nickel-based high-temperature alloy powder on the substrate to form a nickel-based high-temperature alloy deposition layer;

[0029] Depositing Cr metal powder on the surface of the nickel-based high-temperature alloy deposition layer to form a Cr metal deposition layer;

[0030] Depositing V metal powder on the surface of the Cr metal deposition layer to form a V metal deposition layer;

[0031] Titanium alloy powder is deposited on the surface of the V metal deposition layer to form a titanium alloy deposition layer, thereby obtaining a titanium alloy / nickel-based high-temperature alloy bimetallic component.

[0032] In the present invention, unless otherwise specified, the raw materials and equipment used are commercially available products well known in the art.

[0033] In the present invention, the deposition of the following layers all adopts the metal powder laser directed energy deposition technology, and the present invention can use conventional metal powder laser directed energy deposition equipment.

[0034] The present invention deposits nickel-based high-temperature alloy powder on a substrate to form a nickel-based high-temperature alloy deposition layer.

[0035] In the present invention, the substrate is preferably a stainless steel substrate; the particle size of the nickel-based high-temperature alloy powder is preferably 53 to 150 μm. The present invention does not make special requirements on the composition of the nickel-based high-temperature alloy powder, and any nickel-based high-temperature alloy powder known in the art can be used, such as GH4099 and GH4169.

[0036] In the present invention, the conditions for depositing the nickel-based high-temperature alloy powder include: the substrate temperature is preferably 200-1000°C, more preferably 300-800°C, and further preferably 400-600°C; the laser spot diameter is preferably 0.5-3mm, more preferably 2-3mm; the laser power is preferably 350-2600W, specifically 500W, 550W, 800W, 1000W, 1500W, 2000W, 2200W, 2400W, 2600W, which are not listed here; the laser scanning rate is preferably 300-1200mm / min, specifically 300mm / min, 450mm / min, 600mm / min, 800mm / min, 1000mm / min, 1200mm / min, which are not listed here; the single-layer deposition thickness is preferably 0.2-0.5mm.

[0037] In the present invention, the total thickness of the nickel-based high-temperature alloy deposition layer is preferably 5 to 50 mm, more preferably 10 to 30 mm, and further preferably 15 to 20 mm. In the embodiment of the present invention, it is 5 mm or 10 mm.

[0038] After the nickel-based high-temperature alloy deposition layer is formed, the present invention deposits Cr metal powder on the surface of the nickel-based high-temperature alloy deposition layer to form a Cr metal deposition layer.

[0039] In the present invention, the particle size of the Cr metal powder is preferably 53-150 μm. In the present invention, the conditions for depositing the Cr metal powder include: the laser spot diameter is preferably 0.5-3 mm, more preferably 2-3 mm; the laser power is preferably 350-2600 W, specifically 500 W, 550 W, 800 W, 1000 W, 1500 W, 2000 W, 2200 W, 2400 W, 2600 W, which are not listed here; the laser scanning rate is preferably 300-1200 mm / min, specifically 300 mm / min, 450 mm / min, 600 mm / min, 800 mm / min, 1000 mm / min, 1200 mm / min, which are not listed here; the single layer deposition thickness is preferably 0.2-0.5 mm.

[0040] In the present invention, the total thickness of the Cr metal deposition layer is preferably 0.2 to 1 mm, more preferably 0.4 to 0.9 mm, and further preferably 0.5 to 0.7 mm. In an embodiment of the present invention, it is 0.2 mm or 1 mm.

[0041] After forming the Cr metal deposition layer, the present invention deposits V metal powder on the surface of the Cr metal deposition layer to form a V metal deposition layer.

[0042] In the present invention, the particle size of the V metal powder is preferably 53-150 μm. In the present invention, the conditions for depositing the V metal powder include: the laser spot diameter is preferably 0.5-3 mm, more preferably 1-2 mm; the laser power is preferably 350-2600 W, specifically 500 W, 550 W, 800 W, 1000 W, 1500 W, 2000 W, 2200 W, 2400 W, 2600 W, which are not listed here; the laser scanning rate is preferably 300-1200 mm / min, specifically 300 mm / min, 450 mm / min, 600 mm / min, 800 mm / min, 1000 mm / min, 1200 mm / min, which are not listed here; the single layer deposition thickness is preferably 0.2-0.5 mm.

[0043] In the present invention, the total thickness of the V metal deposition layer is preferably 0.2-1 mm, more preferably 0.4-0.9 mm, and further preferably 0.5-0.7 mm. In the embodiment of the present invention, it is 0.2 mm or 0.7 mm.

[0044] After forming the V metal deposition layer, the present invention deposits titanium alloy powder on the surface of the V metal deposition layer to form a titanium alloy deposition layer, thereby obtaining a titanium alloy / nickel-based high-temperature alloy bimetallic component.

[0045] In the present invention, the particle size of the titanium alloy powder is preferably 53-150 μm. The present invention does not make any special requirements on the composition of the titanium alloy powder, and any titanium alloy powder known in the art, such as TA15 and TC4, can be used.

[0046] In the present invention, the conditions of the titanium alloy powder include: the laser spot diameter is preferably 0.5-3 mm, more preferably 1-2 mm; the laser power is preferably 350-2600 W, specifically 500 W, 550 W, 800 W, 1000 W, 1500 W, 2000 W, 2200 W, 2400 W, 2600 W, which are not listed here; the laser scanning rate is preferably 300-1200 mm / min, specifically 300 mm / min, 450 mm / min, 600 mm / min, 800 mm / min, 1000 mm / min, 1200 mm / min, which are not listed here; the single-layer deposition thickness is preferably 0.2-0.5 mm.

[0047] In the present invention, the total thickness of the titanium alloy deposited layer is preferably 5 to 50 mm, more preferably 10 to 40 mm, and further preferably 20 to 30 mm. In the embodiment of the present invention, it is 5 mm or 10 mm.

[0048] The present invention uses a Cr / V bimetallic deposition layer as a connection transition layer and utilizes conventional metal powder laser directional energy deposition equipment to prepare a titanium alloy / nickel-based high-temperature alloy bimetallic structural component with good interface bonding.

[0049] The method for manufacturing titanium alloy / nickel-based high-temperature alloy bimetallic components by laser directional energy deposition of metal powder provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0050] Example 1

[0051] Step 1: Use metal powder laser directed energy deposition equipment, set the spot diameter to 2mm, the laser power to 550W, the laser scanning speed to 450mm / min, control the substrate preheating temperature to 500℃, and deposit GH4099 nickel-based high-temperature alloy powder on the surface of the stainless steel substrate to form a 5mm thick GH4099 high-temperature alloy deposition layer;

[0052] Step 2: Set the spot diameter to 2 mm, the laser power to 550 W, and the laser scanning speed to 450 mm / min. On the basis of the GH4099 nickel-based high-temperature alloy deposition layer obtained in step 1, deposit a layer of pure Cr metal powder to form a 0.2 mm thick pure Cr metal deposition layer.

[0053] Step 3: Set the spot diameter to 2 mm, the laser power to 550 W, and the laser scanning speed to 450 mm / min. On the basis of the pure Cr metal deposition layer obtained in step 2, deposit a layer of pure V metal powder to form a 0.2 mm thick pure V metal deposition layer, and use the Cr / V bimetal deposition layer as a connecting transition layer.

[0054] Step 4: Set the spot diameter to 2 mm, the laser power to 550 W, and the laser scanning speed to 450 mm / min. On the basis of the Cr / V bimetallic deposition layer obtained in step 3, deposit TA15 titanium alloy powder to form a 5 mm thick TA15 titanium alloy deposition layer, and finally obtain a complete titanium alloy / nickel-based high-temperature alloy bimetallic structure.

[0055] The titanium alloy / nickel-based high-temperature alloy bimetallic sample prepared in this embodiment is as follows: Figure 1 As shown in (a), the sample has good formability and no surface macro cracks. The microstructure morphology of the internal interface of the sample is as follows: Figure 2 As shown in the figure, it can be seen that the internal interface of the sample is well bonded, without defects such as cracks and holes. The XRD characterization results of the internal interface of the sample are as follows Figure 3 As shown, the XRD characterization results show that no intermetallic compounds are produced at each interface.

[0056] Example 2

[0057] Step 1: Use metal powder laser directed energy deposition equipment, set the spot diameter to 2mm, the laser power to 550W, the laser scanning speed to 450mm / min, control the substrate preheating temperature to 500℃, and deposit GH4099 nickel-based high-temperature alloy powder on the surface of the stainless steel substrate to form a 10mm thick GH4099 high-temperature alloy deposition layer;

[0058] Step 2: Set the spot diameter to 2 mm, the laser power to 450 W, and the laser scanning speed to 450 mm / min. On the basis of the GH4099 nickel-based high-temperature alloy deposition layer obtained in step 1, deposit a layer of pure Cr metal powder to form a 0.2 mm thick pure Cr metal deposition layer.

[0059] Step 3: Set the spot diameter to 2 mm, the laser power to 450 W, and the laser scanning speed to 450 mm / min. On the basis of the pure Cr metal deposition layer obtained in step 2, deposit a layer of pure V metal powder to form a 0.2 mm thick pure V metal deposition layer, and use the Cr / V bimetal deposition layer as a connecting transition layer.

[0060] Step 4: Set the spot diameter to 2 mm, the laser power to 550 W, and the laser scanning speed to 450 mm / min. On the basis of the Cr / V bimetallic deposition layer obtained in step 3, deposit TA15 titanium alloy powder to form a 10 mm thick TA15 titanium alloy deposition layer, and finally obtain a complete titanium alloy / nickel-based high-temperature alloy bimetallic structure.

[0061] The titanium alloy / nickel-based high-temperature alloy bimetallic sample prepared in this embodiment is as follows: Figure 1 As shown in (b), the sample has good formability and no surface macro cracks.

[0062] Example 3

[0063] Step 1: Use metal powder laser directed energy deposition equipment, set the spot diameter to 3mm, the laser power to 2000W, the laser scanning speed to 1200mm / min, control the substrate preheating temperature to 500℃, and deposit GH4099 nickel-based high-temperature alloy powder on the surface of the stainless steel substrate to form a 5mm thick GH4099 high-temperature alloy deposition layer;

[0064] Step 2: Set the spot diameter to 3 mm, the laser power to 2000 W, and the laser scanning speed to 1200 mm / min. On the basis of the GH4099 nickel-based high-temperature alloy deposition layer obtained in step 1, deposit a layer of pure Cr metal powder to form a 1 mm thick pure Cr metal deposition layer;

[0065] Step 3: Set the spot diameter to 3 mm, the laser power to 2000 W, and the laser scanning speed to 1200 mm / min. On the basis of the pure Cr metal deposition layer obtained in step 2, deposit a layer of pure V metal powder to form a 0.7 mm thick pure V metal deposition layer, and use the Cr / V bimetal deposition layer as a connecting transition layer.

[0066] Step 4: Set the spot diameter to 3mm, the laser power to 2000W, and the laser scanning speed to 1200mm / min. On the basis of the Cr / V bimetallic deposition layer obtained in step 3, deposit TA15 titanium alloy powder to form a 5mm thick TA15 titanium alloy deposition layer, and finally obtain a complete titanium alloy / nickel-based high-temperature alloy bimetallic structure.

[0067] The titanium alloy / nickel-based high-temperature alloy bimetallic sample prepared in this embodiment is as follows: Figure 1 As shown in (c), the sample has good formability and no surface macro cracks.

[0068] Comparative Example 1

[0069] The Cr / V transition layer is omitted.

[0070] Step 1: Use metal powder laser directed energy deposition equipment, set the spot diameter to 2mm, the laser power to 550W, the laser scanning speed to 450mm / min, control the substrate preheating temperature to 500℃, and deposit GH4099 nickel-based high-temperature alloy powder on the surface of the stainless steel substrate to form a 5mm thick GH4099 high-temperature alloy deposition layer;

[0071] Step 2: Set the spot diameter to 2 mm, the laser power to 550 W, and the laser scanning speed to 450 mm / min. On the basis of the GH4099 high-temperature alloy deposition layer obtained in step 1, directly deposit TA15 titanium alloy powder to form a 5 mm thick TA15 titanium alloy deposition layer, and finally obtain a complete titanium alloy / nickel-based high-temperature alloy bimetallic structure.

[0072] The microstructure morphology and XRD characterization results of the internal interface of the titanium alloy / nickel-based high-temperature alloy direct bonding sample are as follows: Figure 4 As shown, the microscopic morphology shows that cracks are generated at the interface, and the XRD characterization results show that a large amount of intermetallic compounds exist at the interface.

[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for manufacturing a titanium alloy / nickel-based high-temperature alloy bimetallic component by laser directed energy deposition of metal powder, characterized in that: The following steps are involved: Depositing nickel-based high-temperature alloy powder on a substrate to form a nickel-based high-temperature alloy deposition layer; Depositing Cr metal powder on the surface of the nickel-based high-temperature alloy deposition layer to form a Cr metal deposition layer; Depositing V metal powder on the surface of the Cr metal deposition layer to form a V metal deposition layer; Titanium alloy powder is deposited on the surface of the V metal deposition layer to form a titanium alloy deposition layer, thereby obtaining a titanium alloy / nickel-based high-temperature alloy bimetallic component.

2. The method according to claim 1, characterized in that The total thickness of the Cr metal deposition layer is 0.2-1 mm.

3. The method according to claim 1, characterized in that The total thickness of the V metal deposition layer is 0.2-1 mm.

4. The method according to claim 1 or 2, characterized in that: The conditions for depositing the Cr metal powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

5. The method according to claim 1 or 3, characterized in that: The conditions for depositing the V metal powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

6. The method according to claim 1, characterized in that The conditions for depositing the nickel-based high-temperature alloy powder include: substrate temperature of 200-1000° C., laser spot diameter of 0.5-3 mm, laser power of 350-2600 W, laser scanning rate of 300-1200 mm / min, and single-layer deposition thickness of 0.2-0.5 mm.

7. The method according to claim 1 or 6, characterized in that: The total thickness of the nickel-based high-temperature alloy deposition layer is 5 to 50 mm.

8. The method according to claim 1, characterized in that The conditions for depositing the titanium alloy powder include: a laser spot diameter of 0.5 to 3 mm, a laser power of 350 to 2600 W, a laser scanning rate of 300 to 1200 mm / min, and a single layer deposition thickness of 0.2 to 0.5 mm.

9. The method according to claim 1 or 8, characterized in that: The total thickness of the titanium alloy deposition layer is 5 to 50 mm.

10. The method according to claim 1, characterized in that The particle sizes of the nickel-based high-temperature alloy powder, the Cr metal powder, the V metal powder and the titanium alloy powder are independently 53 to 150 μm.

Citation Information

Patent Citations

  • Laser manufacturing method for preparing Ni base alloy gradient materials on titanium alloy

    CN105154872A

  • High-temperature-resistant light metal cladding material and preparation method thereof

    CN112497864A

  • Preparation method for manufacturing titanium alloy and nickel-based superalloy functionally graded material

    CN112809007A

  • Integrated additive manufacturing method for heterogeneous metal bionic component

    CN114713849A

  • Strengthening method for SLM additive manufacturing interface of stainless steel-titanium alloy dissimilar metal

    CN118305330A