Electric arc additive manufacturing method for pulse laser beam in-situ impact pasty area

The use of a pulsed laser beam to refine the mushy zone in arc additive manufacturing addresses issues of coarse grains and defects by transforming columnar crystals into finer equiaxed crystals, enhancing the mechanical properties and welding quality.

CN119057176APending Publication Date: 2024-12-03NANJING UNIV OF SCI & TECH

Patent Information

Application Number
CN202310649063.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Conventional arc additive manufacturing processes face issues with high energy density, large temperature gradients, coarse weld grain structures, and the propensity for defects such as cracks due to uneven thermal processes and grain structure complexity.

Method used

A method involving a pulsed laser beam in-situ impacting the mushy zone of the molten pool, using a continuous pulse laser with specific parameters to disturb the mushy zone, refining the grain structure by breaking up columnar crystals into finer equiaxed crystals, thereby improving the microstructure and mechanical properties.

Benefits of technology

The method achieves refined weld grains, reduces thermal crack sensitivity, and enhances the mechanical properties of the weld structure, ensuring improved welding quality and efficiency while minimizing defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057176A_ABST
    Figure CN119057176A_ABST
Patent Text Reader

Abstract

The invention discloses an electric arc additive manufacturing method for pulse laser beam in-situ impact on a pasty area, which comprises the following steps of: establishing a related calculation model based on Fluent software, and carrying out visual analysis on an additive process to obtain parameters of a molten pool and the pasty area in the additive process; setting a relative distance between the arc gun head and the laser head and determining related experimental parameters; the laser continuously impacts the paste area of the molten pool at a proper pulse waveform and a certain pulse frequency while the electric arc is added. According to the method, continuous pulse laser shock is conducted on a paste area of a molten pool in the electric arc material increasing process, grains in the material increasing area are refined, and the comprehensive mechanical property of a component is optimized; and the pulse laser is added to smash columnar crystals formed in the pasty area, so that the columnar crystals are subjected to secondary nucleation growth and further grow into relatively fine isometric crystals, and finally, the aims of refining crystal grains and improving the strength, wear resistance and corrosion resistance of the sample are fulfilled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of arc additive manufacturing, relates to an arc additive manufacturing method, and relates to an arc additive manufacturing method in which a pulsed laser beam in-situ impacts a mushy area. Background Art

[0002] Additive manufacturing technology was first proposed in the United States during the economic crisis in the late 1970s to revitalize the real economy. It was widely used in the mid-1980s. It is an emerging processing technology developed on the basis of traditional material cutting processing technology. Additive manufacturing technology is different from the previous equal material manufacturing mode and cutting and subtractive manufacturing mode of using raw materials for casting. Additive manufacturing technology is a technology that uses materials "layer by layer" and "bottom-up" to manufacture solid parts, realizing the transformation of processed products to personalized and customized. The principle of additive manufacturing technology is the same as that of 3D printing technology. Its basic process is as follows: first, design a solid model on a computer simulation software; second, divide the model from bottom to top to discretize the solid model into a series of two-dimensional models; finally, stack the discretized two-dimensional model layer by layer to generate the required three-dimensional solid model.

[0003] Arc additive manufacturing technology uses arc as a heat source and adopts a layer-by-layer surfacing method to manufacture metal components. Because of its high heat input, high forming efficiency, low equipment cost, and no volume limit on the formed components, it is often used for additive manufacturing of large components. However, due to the high energy, high energy density, and fast forming speed of the arc, there are problems such as coarse grains and stress concentration in the additive structure during the arc additive process, and defects such as pores and cracks are prone to occur. It is necessary to adjust and improve the process parameters and methods to avoid the generation of additive defects.

[0004] The mushy zone of the molten pool is the solid-liquid coexistence zone in the latter half of the molten pool. As the heat source moves forward, the temperature of this area continues to decrease, and the front of the solid-liquid interface continues to advance. The dendrites generated by the solid phase grow forward, and at the same time, the dendrites overlap each other to form a solid phase skeleton; with the continuous growth of dendrites and the rapid cooling and solidification of the molten pool, the temperature decreases in the late cooling and solidification, and the already formed solid phase skeleton begins to shrink; since the molten pool is cooled from the outside to the inside, it is a non-uniform shrinkage, so stress and deformation are generated in the mushy zone; when the deformation exceeds the deformation capacity limit of the alloy in the brittle temperature range, it will tear the grain boundary to form a gap; as the temperature drops, it becomes more difficult for the liquid metal to reflux and heal. When the intercrystalline liquid film is too narrow or discontinuous, and the gap cannot be filled by liquid metal in time, a crack defect will be formed. Therefore, the mushy zone of the molten pool is a sensitive area for the formation of thermal cracks.

[0005] In the process of arc additive, the thermal process is much more complicated than the general heat treatment process. The thermal process of arc additive is similar to that of arc welding. The arc heat source is locally concentrated and instantaneous. The temperature of the position swept by the heat source rises sharply, and the temperature gradient is large. After leaving, the temperature cools down again, and the heating and cooling are extremely uneven. The liquid metal in the molten pool is in a state of intense motion, and its heat transfer mode is mainly convection. The outer area of ​​the molten pool is mainly solid-state heat conduction, and there is also radiation heat dissipation. In addition, unlike arc welding, the arc additive process is a surfacing process. Each weld of the subsequent additive will transfer heat to each weld of the previous additive, which is equivalent to a heat treatment process. In general, the heat transfer process of arc additive is very complicated. The grain structure of the weld produced under this condition is relatively coarse and complex. Therefore, it is extremely important to study and refine the grain structure of the arc additive weld area.

[0006] Wang Yipeng et al. disclosed in their Chinese invention patent entitled “A MIG arc twin-wire low heat input additive manufacturing method for scanning laser-assisted shaping of molten pool” and publication number CN115008017A a MIG arc twin-wire low heat input additive manufacturing method for scanning laser-assisted shaping of molten pool, which realizes dynamic shaping of the morphology and size of the molten pool; its limitation is that the structure of the formed part is not changed, and there is a limitation on the improvement of the performance of the formed part.

[0007] Yi Hao et al. disclosed a device and method for additive manufacturing using composite arc of laser impact stirring a molten pool with variable orientation in a Chinese invention patent with the invention name “A device and method for additive manufacturing using composite arc of laser impact stirring a molten pool with variable orientation” and publication number CN114951905A, which realized additive manufacturing using composite arc of laser impact stirring a molten pool with different orientations; however, the disadvantage is that the energy of continuous laser is too concentrated, resulting in high energy consumption, which can easily cause splashing during the additive process, leading to severe burning of the material. Summary of the invention

[0008] In view of the defects generated in the arc additive manufacturing process mentioned above, the technical problem to be solved by the present invention is: under conventional arc additive manufacturing, the arc energy is high, the energy density is large, the temperature gradient is large, the weld grain structure formed is coarse, the organizational properties are uneven, and defects such as cracks are easily generated.

[0009] In order to solve the above problems, the present invention provides an arc additive manufacturing process method in which a pulsed laser beam in-situ impacts a mushy zone, and a continuous pulse laser with a suitable pulse waveform and pulse frequency impacts the mushy zone of the molten pool, thereby bringing continuous heat and mass disturbance to the mushy zone of the molten pool, breaking up the coarse columnar crystals in the mushy zone of the molten pool, causing secondary nucleation and growing into relatively fine equiaxed crystals, thereby improving the microstructure inside the molten pool, thereby improving its comprehensive mechanical properties, and comprising the following steps:

[0010] Step 1: According to the selected additive process parameters, a relevant model is established through Fluent software to visualize the additive process, obtain the size and shape parameters of the molten pool and the mushy zone at different times during the additive process, and the distance between the molten pool and the mushy zone, and then determine the pulse laser action position;

[0011] Step 2: Select a suitable additive substrate and welding wire, grind and clean the substrate surface, and clamp the substrate onto a horizontal workbench;

[0012] Step 3: Install a controllable movable fixture and laser on the arc gun head, adjust the circuit, and achieve the synergistic effect of the arc and laser through programming and signal interaction.

[0013] Step 4, according to the computer numerical simulation results, adjust the relative distance between the arc gun head and the laser head and the angle between the arc gun head and the substrate, and adjust the wire dry extension amount, so that the position distance between the laser irradiation point and the welding wire is a, the distance between the welding wire and the substrate is b, the angle between the arc and the substrate is α, and the angle between the laser and the substrate is β;

[0014] Step 5: Setting arc additive process parameters, which include arc voltage, arc current, welding speed, arc shielding gas flow rate and wire feeding speed;

[0015] Step 6, setting pulse laser related process parameters, which include laser power, defocus, spot diameter, laser movement speed, pulse period, pulse width, pulse interval and pulse frequency;

[0016] Step 7: Turn on the arc and start the additive process according to the preset trajectory. At the same time, the laser emits the laser. The laser and the arc are kept at a certain distance and continuously impact the mushy area of ​​the molten pool. The additive process is completed according to the preset trajectory. The arc is turned off and the laser is turned off so that the laser can impact the entire cladding layer.

[0017] Furthermore, in step 1, a relevant calculation model is established based on the Fluent software to visualize the additive process. By setting the corresponding additive process parameters, the size and shape parameters of the molten pool and the mushy zone of the additive process at different times and the distance between the molten pool and the mushy zone are obtained. The distance between the molten pool and the mushy zone is used to determine the relative distance between the laser irradiation point and the end of the welding wire, and then the action position of the pulsed laser is determined.

[0018] Further, in step 2, the substrate is a 304 stainless steel plate, the welding wire is a CrNi199 stainless steel welding wire, the welding wire diameter is 0.8-1.6 mm, the chemical composition of the 304 stainless steel plate is: C≤0.08%, Si≤1.00%, Mn≤2.00%, 8%≤Ni≤15%, 18%≤Cr≤20%, and the balance is Fe, and the chemical composition of the CrNi199 stainless steel welding wire is C≤0.08%, Si≤1.00%, Mn≤2.00%, P≤0.035%, S≤0.030%, Ni: 8.00%-10.50%, Cr: 18.00%-20.00%, and the balance is Fe.

[0019] Furthermore, in step 3, the combined effect of laser and arc is achieved by controlling the movable fixture, and the connection circuit of the working robot is further adjusted to achieve the synergistic effect of arc and laser through programming and signal interaction.

[0020] Furthermore, in step 4, the moving paths of the laser and the arc are kept consistent and coincide with the center line of the welding trajectory. The laser and the arc are kept at a certain distance to ensure that the arc is in front and the laser is behind, so that the pulsed laser can continuously act on the molten pool paste area, the angle α between the arc and the substrate is 30°~60°, the angle β between the laser and the substrate is 80°~100°, and the following conditions are met: 0°≤α<β≤180°; the dry elongation of the welding wire l is 8~10mm, the distance b between the welding wire and the substrate is 0.5~3mm, and the position distance a between the laser irradiation point and the end of the welding wire is 0.5~7mm, and its specific size is obtained by computer simulation in step 1, a changes dynamically with time, and the controllable movable fixture is driven to move by a computer-controlled motor, so that the laser can continuously impact the molten pool paste area during the additive process, and the following conditions are met: d<b≤a<lsinα.

[0021] Further, in step 5, the arc voltage U is 18-25V, the current I is 170-190A, the arc movement speed v1 is 0.18-0.54m / min, the arc shielding gas is vol% 99.99Ar, the shielding gas flow rate v4 is 10-18L / min, and the wire feeding speed v3 is 4.8-7.4m / min.

[0022] Further, in step 6, the laser power P is 400~1200W, the defocus amount D is -12~2mm, the spot diameter d is 0.8~1.4mm, the laser movement speed v2 is 0.18~0.54m / min, the pulse frequency f=1 / pulse period T, the pulse period T=pulse width T1+pulse interval T2, and the following conditions v1=v2<0.4(v1+v2)v3 are satisfied, and the pulse waveforms include rectangular wave, sawtooth wave, triangular wave, spike wave, step wave, etc.

[0023] Furthermore, in step 7, after the additive process is completed according to the preset trajectory, the arc is extinguished first and then the laser is turned off, so that the pulsed laser can impact the entire weld.

[0024] The present invention discloses a pulse laser and arc additive composite manufacturing system, which is applied to the above-mentioned arc additive manufacturing process method of in-situ pulse laser beam impacting a mushy area, and specifically includes:

[0025] A controllable movable fixture is used to fix the laser on the arc gun head to make them work together;

[0026] An arc welder, used in conjunction with the laser to melt the welding wire and substrate;

[0027] A laser is used to emit a pulsed laser beam with a power of 400 to 1200 W to act on the mushy area of ​​the molten pool;

[0028] A wire feeding device, used for feeding the welding wire so that it melts together with the substrate to form a molten pool;

[0029] Gas supply device, used to supply protective gas to make the weld shape beautiful, reduce defects and protect the laser head;

[0030] By fixing the arc welding machine and the laser with a controllable movable fixture, and in cooperation with the gas supply device and the wire supply device, the required components are surfacing-welded on the substrate according to the planned welding path, and the required structural parts are formed layer by layer. Compared with the prior art, the present invention has at least the following advantages:

[0031] The present invention is different from traditional arc additive manufacturing in that it uses continuous pulse laser to impact the mushy zone of the molten pool to achieve the purpose of grain refinement in the weld area during the additive welding process; a controllable movable fixture is used to control the laser and the arc gun head to maintain a certain distance and work together at the same speed, so that the pulsed laser beam continuously impacts the mushy zone in situ during the arc additive process, and the coarse columnar crystals in the mushy zone are broken up by laser impact, and the broken columnar crystals undergo secondary nucleation and growth to form relatively fine equiaxed crystals, thereby achieving the purpose of refining the weld structure, inducing residual stress, reducing thermal crack sensitivity, and reducing the generation of defects such as cracks, thereby achieving the strengthening effect of laser on the weld structure.

[0032] Compared with common additive manufacturing technology, the present invention achieves the effect of refining weld grains by adding pulsed laser while realizing additive manufacturing, thereby ensuring welding quality and efficiency, and avoiding the decrease in welding efficiency seen in other studies.

[0033] The pulse laser waveform of the present invention is diverse, and the waveform can be selected according to actual conditions, with high flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1This is a diagram of a laser arc compound device.

[0035] Figure 2 It is a composite schematic diagram of the laser head and the welding gun head.

[0036] Figure 3 It is a schematic diagram of pulse laser waveform.

[0037] Figure 4 This is a schematic diagram of the arc laser action position.

[0038] Figure 5 This is a metallographic microstructure diagram of the cross section of the cladding layer in Example 1 with only arc action.

[0039] Figure 6 This is a metallographic microstructure diagram of the cross section of the cladding layer in Example 1 when the arc and pulse laser act simultaneously.

[0040] Figure 1 Middle: 1. Power supply; 2. Shielding gas cylinder; 3. Laser controller; 4. Arc controller; 5. Substrate; 6. Workbench; 7. Additive area; 8. Mobile fixture; 9. Shielding gas nozzle; 10. Laser head; 11. Arc gun head.

[0041] Figure 2 Middle: 5, substrate; 6, workbench; 9, shielding gas nozzle; 10, laser head; 11, arc gun head; a, distance between laser irradiation point and end of welding wire; b, distance between welding wire and substrate; α, angle between arc and substrate; β, angle between laser and substrate; arrow direction is additive direction.

[0042] Figure 3 Chinese: P, power; P m Peak power; T, pulse period; T1 pulse width; T2 pulse interval; t time.

[0043] Figure 4 Middle: 5, substrate; 10, laser head; 11, arc gun head; 12, mushy area; 13, molten pool; a, the position distance between the laser irradiation point and the end of the welding wire. Specific implementation plan

[0044] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0045] Example 1

[0046] In this embodiment, the arc material addition method of in-situ impact of a pulsed laser beam on a mushy zone is specifically performed in the following steps:

[0047] Step 1: Set the additive process parameters, arc current 160A, arc voltage 24.8V, build the relevant model through Fluent software, visualize the additive process, and obtain the size and shape parameters of the molten pool and the mushy zone at different times in the additive process, as well as the distance between the molten pool and the mushy zone, such as Figure 4 As shown, the distance between the molten pool and the mushy zone is determined to determine the position distance a between the laser irradiation point and the end of the welding wire, and the wire spacing size a is 2 mm.

[0048] Step 2: Prepare 304 steel plate of 200*150*8mm, prepare CrNi199 stainless steel welding wire of 1.2mm diameter, prepare vol% 99.99Ar as arc shielding gas, grind and clean the surface of the substrate to remove the surface oxide layer and oil stains, and apply four cylindrical clamps with a diameter of 15mm to the substrate along the direction of gravity. The clamping force is 2kN to fix the substrate on the workbench. The chemical composition of 304 stainless steel plate measured by a handheld element analyzer is: C: 0.08%, Si: 1.00%, Mn: 2.00%, Ni: 10%, Cr: 19%, and the balance is Fe. The chemical composition of CrNi199 stainless steel welding wire is C: 0.08%, Si: 1.00%, Mn: 2.00%, P: 0.035%, S: 0.030%, Ni: 9.5.00%, Cr: 19.00%, and the balance is Fe.

[0049] Step 3: Edit the program so that the moving paths of the laser and arc are consistent and coincide with the center line of the welding trajectory, ensuring that the arc is in front and the laser is behind, so that the pulsed laser acts continuously on the mushy area of ​​the molten pool, the angle α between the arc and the substrate: 60°, the angle β between the laser and the substrate: 90°, the dry elongation of the welding wire l: 10mm, the distance between the welding wire and the substrate b: 2mm, the position distance between the laser irradiation point and the end of the welding wire a: 2mm.

[0050] Step 4: Set the arc additive current I: 160A, arc voltage U: 24.8V, wire feeding speed v3: 6.3m / min, shielding gas flow v4: 15L / min, arc welding speed v1: 0.36m / min.

[0051] Step 5: Set the laser power P: 500W, defocus D: -5mm, spot diameter d: 1.15mm, laser movement speed v2: 0.36m / min, pulse period T: 2s, pulse width T1: 0.5s, and the pulse waveform is a rectangular wave, such as Figure 4 shown.

[0052] Step 6: Turn on the arc and laser at the same time. While the arc is being added, the pulsed laser beam emitted by the laser head continuously impacts the paste area at a certain period to complete the addition process according to the preset trajectory. After the addition is completed, the arc is extinguished first, and then the laser is turned off.

[0053] Step 7: Follow the above steps to complete the additive process according to the preset trajectory, turn off the arc, and turn off the laser so that the laser can impact the entire weld.

[0054] Step 8: After surface cleaning, the cross-sectional microstructure of the cladding layer with arc and laser acting simultaneously and arc acting alone is observed. The cladding layer structure is mainly composed of austenite columnar crystals, δ ferrite dendrites and σ phases growing perpendicular to the fusion line. The δ ferrite is long and evenly distributed in the austenite grains. The grain size of the cladding layer with arc and pulsed laser acting simultaneously is finer, about 10.6μm; the grain size of the cladding layer with arc acting alone is about 11.2μm. Small and shallow dimples are distributed on the tensile fracture surface of the cross-sectional cladding layer, and the tensile fracture mode is ductile fracture. The tensile strength of the cladding layer with the simultaneous action of arc and pulse laser is 526MPa, the yield strength is 198Mpa, and the elongation is 19.6%; the tensile strength of the cladding layer with only the action of arc is 522MPa, the yield strength is 195Mpa, and the elongation is 19.2%. Through comparative analysis, it can be seen that after adding pulse laser, the strength of the additively manufactured sample is significantly increased, the toughness is enhanced, and the performance is improved.

[0055] Example 2

[0056] In this embodiment, the arc material addition method of in-situ impact of a pulsed laser beam on a mushy zone is specifically performed in the following steps:

[0057] Step 1: Set the additive process parameters, arc current 160A, arc voltage 24.8V, build the relevant model through Fluent software, visualize the additive process, and obtain the size and shape parameters of the molten pool and the mushy zone at different times in the additive process, as well as the distance between the molten pool and the mushy zone, such as Figure 4 As shown, the distance between the molten pool and the mushy zone is determined to determine the position distance a between the laser irradiation point and the end of the welding wire, and the wire spacing size a is 2 mm.

[0058] Step 2: Prepare 304 stainless steel plate of 200*150*8mm, prepare CrNi199 stainless steel welding wire of 1.2mm diameter, prepare vol% 99.99Ar as arc shielding gas, grind and clean the surface of the substrate to remove the surface oxide layer and oil stains, and apply four cylindrical clamps with a diameter of 15mm to the substrate along the direction of gravity. The clamping force is 2kN to fix the substrate on the workbench. The chemical composition of 304 stainless steel plate measured by a handheld element analyzer is: C: 0.08%, Si: 1.00%, Mn: 2.00%, Ni: 10%, Cr: 19%, and the balance is Fe. The chemical composition of CrNi199 stainless steel welding wire is C: 0.08%, Si: 1.00%, Mn: 2.00%, P: 0.035%, S: 0.030%, Ni: 9.5.00%, Cr: 19.00%, and the balance is Fe.

[0059] Step 3: Edit the program so that the moving paths of the laser and arc are consistent and coincide with the center line of the welding trajectory, ensuring that the arc is in front and the laser is behind, so that the pulsed laser acts continuously on the mushy area of ​​the molten pool, the angle α between the arc and the substrate: 60°, the angle β between the laser and the substrate: 90°, the dry elongation of the welding wire l: 10mm, the distance between the welding wire and the substrate b: 2mm, the position distance between the laser irradiation point and the end of the welding wire a: 2mm.

[0060] Step 4: Set the arc additive current I: 160A, arc voltage U: 24.8V, wire feeding speed v3: 6.3m / min, shielding gas flow v4: 15L / min, arc welding speed v1: 0.36m / min.

[0061] Step 5: Set the laser power P: 550W, defocus D: -50mm, spot diameter d: 1.15mm, laser movement speed v2: 0.36m / min, pulse period T: 2s, pulse width T1: 0.6s, and the pulse waveform is a rectangular wave, such as Figure 3 shown.

[0062] Step 6: Turn on the arc and laser at the same time. While the arc is being added, the pulsed laser beam emitted by the laser head continuously impacts the paste area at a certain period to complete the addition process according to the preset trajectory. After the addition is completed, the arc is extinguished first, and then the laser is turned off.

[0063] Step 7: Follow the above steps to complete the additive process according to the preset trajectory, turn off the arc, and turn off the laser so that the laser can impact the entire weld.

[0064] Step 8: After surface cleaning, the cross-sectional microstructure of the cladding layer with arc and pulse laser acting simultaneously and arc acting alone is observed. The cladding layer structure is mainly composed of austenite columnar crystals, δ ferrite dendrites and σ phases growing perpendicular to the fusion line. The δ ferrite is long and evenly distributed in the austenite grains. The grain size of the cladding layer with arc and pulse laser acting simultaneously is finer, about 9.6μm; the size of the cladding layer with arc acting alone is about 10.2μm. Small and shallow dimples are distributed on the surface of the tensile fracture of the cross-sectional cladding layer, and the tensile fracture mode is ductile fracture. The tensile strength of the cladding layer with arc and pulse laser acting simultaneously is 529MPa, the yield strength is 203Mpa, and the elongation is 20.4%; the tensile strength of the cladding layer with arc acting alone is 522MPa, the yield strength is 195Mpa, and the elongation is 19.2%; through comparative analysis, it can be seen that the strength of the additive sample is significantly increased after adding pulse laser, the toughness is enhanced, and the performance is improved.

[0065] Example 3

[0066] In this embodiment, the arc material addition method of in-situ impact of a pulsed laser beam on a mushy zone is specifically performed in the following steps:

[0067] Step 1: Set the additive process parameters, arc current 160A, arc voltage 24.8V, build the relevant model through Fluent software, visualize the additive process, and obtain the size and shape parameters of the molten pool and the mushy zone at different times in the additive process, as well as the distance between the molten pool and the mushy zone, such as Figure 4 As shown, the distance between the molten pool and the mushy zone is determined to determine the position distance a between the laser irradiation point and the end of the welding wire, and the wire spacing size a is 2 mm.

[0068] Step 2: Prepare 304 stainless steel plate of 200*150*8mm, prepare CrNi199 stainless steel welding wire of 1.2mm diameter, prepare vol% 99.99Ar as arc shielding gas, grind and clean the surface of the substrate to remove the surface oxide layer and oil stains, and apply four cylindrical clamps with a diameter of 15mm to the substrate along the direction of gravity. The clamping force is 2kN to fix the substrate on the workbench. The chemical composition of 304 stainless steel plate measured by a handheld element analyzer is: C: 0.08%, Si: 1.00%, Mn: 2.00%, Ni: 10%, Cr: 19%, and the balance is Fe. The chemical composition of CrNi199 stainless steel welding wire is C: 0.08%, Si: 1.00%, Mn: 2.00%, P: 0.035%, S: 0.030%, Ni: 9.5.00%, Cr: 19.00%, and the balance is Fe.

[0069] Step 3: Edit the program so that the moving paths of the laser and arc are consistent and coincide with the center line of the welding trajectory, ensuring that the arc is in front and the laser is behind, so that the pulsed laser acts continuously on the mushy area of ​​the molten pool, the angle α between the arc and the substrate: 60°, the angle β between the laser and the substrate: 90°, the dry elongation of the welding wire l: 10mm, the distance between the welding wire and the substrate b: 2mm, the position distance between the laser irradiation point and the end of the welding wire a: 2mm.

[0070] Step 4: Set the arc additive current I: 160A, arc voltage U: 24.8V, wire feeding speed v3: 6.3m / min, shielding gas flow v4: 15L / min, arc welding speed v1: 0.36m / min.

[0071] Step 5: Set the laser power P: 600W, defocus D: -10mm, spot diameter d: 1.15mm, laser movement speed v2: 0.36 / min, pulse period T: 2s, pulse width T1: 0.7s, and the pulse waveform is a rectangular wave, such as Figure 3 shown.

[0072] Step 6: Turn on the arc and laser at the same time. While the arc is being added, the pulsed laser beam emitted by the laser head continuously impacts the paste area at a certain period to complete the addition process according to the preset trajectory. After the addition is completed, the arc is extinguished first, and then the laser is turned off.

[0073] Step 7: Follow the above steps to complete the additive process according to the preset trajectory, turn off the arc, and turn off the laser so that the laser can impact the entire weld.

[0074] Step 8: After surface cleaning, the cross-sectional microstructure of the cladding layer with arc and pulse laser acting simultaneously and arc acting alone is observed. The cladding layer structure is mainly composed of austenite columnar crystals, δ ferrite dendrites and σ phases growing perpendicular to the fusion line. The δ ferrite is long and evenly distributed in the austenite grains. The grain size of the cladding layer with arc and pulse laser acting simultaneously is finer, about 10μm; the size of the cladding layer with arc acting alone is about 10.8μm. Small and shallow dimples are distributed on the surface of the tensile fracture of the cross-sectional cladding layer, and the tensile fracture mode is ductile fracture. The cladding layer with arc and pulse laser acting simultaneously has a tensile strength of 535MPa, a yield strength of 214Mpa, and an elongation of 21.3%; the cladding layer with arc acting alone has a tensile strength of 522MPa, a yield strength of 195Mpa, and an elongation of 19.2%; through comparative analysis, it can be seen that the strength of the additive sample has been significantly increased after adding pulse laser, the toughness has been enhanced, and the performance has been improved.

Claims

1. An arc additive manufacturing method using a pulsed laser beam to impact a mushy zone in situ, It is characterized in that Pulse laser is used to impact the molten pool to strengthen the weld metal. A calculation model is established based on Fluent software to visualize the additive process. By changing the corresponding additive process parameters, the size and shape parameters of the molten pool and the mushy area of ​​the additive process at different times are obtained. Under the heat of the arc, the welding wire and the substrate melt to form a molten pool, and the wire feeding device continuously feeds the welding wire into the molten pool. At the same time, the laser and the arc are kept at a certain distance. The pulse waveform and pulse frequency are selected to continuously impact the mushy area of ​​the molten pool, and the molten pool metal cools and solidifies and spreads on the substrate along the specified route, and the required components are formed by surfacing layer by layer.

2. The arc additive manufacturing method of claim 1 wherein the pulsed laser beam in-situ impacts the mushy zone. It is characterized in that The specific steps include: Step 1: According to the selected additive process parameters, a relevant model is established through Fluent software to visualize the additive process, obtain the size and shape parameters of the molten pool and the mushy zone at different times during the additive process, and the distance between the molten pool and the mushy zone, and then determine the pulse laser action position; Step 2: Select a suitable additive substrate and welding wire, grind and clean the substrate surface, and clamp the substrate onto a horizontal workbench; Step 3: Install a controllable movable fixture and a laser on the arc gun head, adjust the circuit, and realize the synergistic effect of the arc and the laser through programming and signal interaction; Step 4, according to the computer numerical simulation results, adjust the relative distance between the arc gun head and the laser head and the angle between the arc gun head and the substrate, and adjust the wire dry extension amount, so that the position distance between the laser irradiation point and the welding wire is a, the distance between the welding wire and the substrate is b, the angle between the arc and the substrate is α, and the angle between the laser and the substrate is β; Step 5: Set the arc additive process parameters, which include arc voltage, arc current, welding speed, shielding gas flow rate and wire feeding speed; Step 6, setting pulse laser related process parameters, which include laser power, defocus, spot diameter, laser movement speed, pulse period, pulse width, pulse interval and pulse frequency, and pulse waveform; Step 7: Turn on the arc and start the additive process according to the preset trajectory. At the same time, the laser emits the laser. The laser and the arc are kept at a certain distance and continuously impact the mushy area of ​​the molten pool. The additive process is completed according to the preset trajectory. The arc is turned off and the laser is turned off so that the laser can impact the entire cladding layer.

3. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that Based on the Fluent software, a relevant calculation model was established to visualize the additive process. By setting the corresponding additive process parameters, the size and shape parameters of the molten pool and the pasty zone in the additive process at different times and the distance between the molten pool and the pasty zone were obtained. The distance between the molten pool and the pasty zone was used to determine the relative distance between the laser irradiation point and the end of the welding wire, and then the action position of the pulsed laser was determined.

4. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 2, the substrate is a 304 stainless steel plate, the welding wire is a CrNi199 stainless steel welding wire, the diameter of the welding wire size is 0.8-1.6 mm, the chemical composition of the 304 stainless steel plate is: C≤0.08%, Si≤1.00%, Mn≤2.00%, 8%≤Ni≤15%, 18%≤Cr≤20%, and the balance is Fe. The chemical composition of the CrNi199 stainless steel welding wire is C≤0.08%, Si≤1.00%, Mn≤2.00%, P≤0.035%, S≤0.030%, Ni: 8.00%-10.50%, Cr: 18.00%-20.00%, and the balance is Fe.

5. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 3, the pulse laser and arc additive composite manufacturing system used includes a controllable movable fixture, an arc welder, a laser, a wire feeder, and a gas feeder. The controllable movable fixture is used to fix the arc welder and the laser, further adjust the connection circuit of the working robot, and realize the synergistic effect of the arc and the laser through programming and signal interaction; the arc welder is used to cooperate with the laser to melt the welding wire and the substrate; the laser is used to emit a pulsed laser beam with a power of 400 to 1200W, acting on the mushy area of ​​the molten pool; the wire feeder is used to feed the welding wire so that it melts together with the substrate to form a molten pool; the gas feeder is used to feed the protective gas to make the weld shape beautiful, reduce defects, and protect the laser head.

6. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 4, the moving paths of the laser and the arc are consistent and coincide with the center line of the welding trajectory. The laser and the arc are kept at a certain distance to ensure that the arc is in front and the laser is behind, so that the pulsed laser can continuously act on the molten pool paste area, the angle α between the arc and the substrate is 30°~60°, the angle β between the laser and the substrate is 80°~100°, and the following conditions are met: 0°≤α<β≤180°; the dry extension of the welding wire l is 8~10mm, the distance b between the welding wire and the substrate is 0.5~3mm, and the position distance a between the laser irradiation point and the end of the welding wire is 0.5~7mm, and its specific size is obtained by computer simulation in step 1, a changes dynamically with time, and the controllable movable fixture is driven to move by controlling the motor, so that the laser can continuously impact the molten pool paste area during the additive process, and the following conditions are met: d<b≤a<lsinα.

7. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 5, the arc voltage U is 18-25V, the current I is 170-190A, and the arc moving speed v 1 is 0.18~0.54m / min, arc shielding gas is vol%99.99Ar, shielding gas flow rate v 4 is 10-18 L / min, the wire feeding speed v 3 4.8~7.4m / min.

8. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 6, the laser power P is 400-1200W, the defocus D is -12-2mm, the spot diameter d is 0.8-1.4mm, and the laser movement speed v is 2 0.18~0.54m / min, pulse frequency f=1 / pulse period T, pulse period T=pulse width T 1 + Pulse gap T 2 , and the following conditions are met 1 =v 2 <0.4(v 1 +v 2 )v 3 The pulse waveforms include rectangular wave, sawtooth wave, triangle wave, spike wave and step wave.

9. The arc additive manufacturing method of claim 1 wherein a pulsed laser beam in-situ impacts a mushy zone. It is characterized in that In step 7, after the additive process is completed according to the preset trajectory, the arc is extinguished first and then the laser is turned off so that the pulsed laser can impact the entire weld.

Citation Information

Patent Citations

  • Direction-changing laser shock stirring molten pool composite electric arc additive manufacturing device and method

    CN114951905A

  • MIG electric arc double-wire low-heat-input additive manufacturing method for scanning laser-assisted shaping molten pool

    CN115008017A

Cited By

  • Laser-electric arc hybrid welding process for stainless steel ferrule joint

    CN120755512A