Friction stir welding method for integrated die-casting magnesium alloy battery box
Through the integrated friction stir welding method of die-cast magnesium alloy battery box, the problems of many welding positions and poor quality of traditional battery box are solved, and the effects of small welding deformation, few defects and high strength are achieved.
Patent Information
- Application Number
- CN202411191504.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional battery boxes are mostly made of steel or aluminum profiles, with many welding locations and poor product quality, resulting in large deformation of welding, low connection strength and complicated processes.
The friction stir welding method of integrated die-cast magnesium alloy battery box is adopted, and sandpaper grinding and cleaning, multi-point fixing, reasonable welding sequence and parameter design are used, and the mixing head is used for welding, and X-ray flaw detection is carried out to ensure quality.
It reduces welding deformation, improves overall quality, reduces defect rate, meets production needs, and increases welding strength by half.
Smart Images

Figure CN119057202A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a friction stir welding method for an integrated die-cast magnesium alloy battery box, belonging to the technical field of metal material welding. Background Art
[0002] In recent years, new energy vehicles have risen strongly, and the improvement of new energy vehicle range has forced the development of lightweight body. Friction stir welding (FSW) [1,2] is a new solid-phase joining method invented by the British Welding Research Institute in 1991. It uses friction heat and plastic deformation heat as welding heat sources. It has the advantages of low welding cost, high welding efficiency, environmental protection, and no melting of the parent material during welding. It is especially suitable for the same or different welding of lightweight alloys such as aluminum and magnesium [3], providing a new welding technology for lightweight application fields. Traditional battery boxes are mostly welded from steel or aluminum profiles. There are many welding positions and the product quality is large, so the welding deformation is large, correction is required after welding, the connection strength is low, and the process is complicated. Summary of the invention
[0003] The purpose of the present invention is to solve the problems that most of the existing traditional battery cases are welded together from steel or aluminum profiles, have many welding positions and large product quality, resulting in large welding deformation, need for correction after welding, low connection strength and complicated procedures, and propose a stir friction welding method for an integrated die-cast magnesium alloy battery case.
[0004] The problem to be solved by the present invention is achieved by the following technical solutions:
[0005] A friction stir welding method for an integrated die-cast magnesium alloy battery case, comprising:
[0006] Step S1, grinding the front and back surfaces of the magnesium alloy profile cover plate and the welds of the magnesium alloy box integrated water jacket with sandpaper, and cleaning with alcohol and acetone after grinding;
[0007] Step S2, placing the box body on a special tooling for the friction stir welding machine, placing the cover plate on the welding bead of the box body, and fixing the cover plate and the box body with a clamp;
[0008] Step S3, the clamp is fixed at multiple points on the lap weld of the outermost circle, and during welding, the multiple-point clamp will be lifted up and then lowered to fix and clamp in sequence as the stirring head passes by;
[0009] Step S4, the flat-head stirring head is first fixed by multi-point welding on the outermost weld bead, and then pre-welded for one circle;
[0010] Step S5, after replacing the pointed stirring head, welding is performed from the outermost circle, and then welding is performed according to the designed welding sequence and welding process parameters;
[0011] Step S6, the stirring needle is pulled out without rotation at the arc closing point of all welds, and the flat-head stirring head is replaced after welding, and the keyhole is filled with a small piece of the same magnesium plate;
[0012] Step S7, after welding, the burrs are cleaned and then X-ray flaw detection is performed.
[0013] Preferably, in step S1, the sandpaper used is 400#-1000#.
[0014] Preferably, in step S1, the thickness of the magnesium alloy profile cover plate is 2 mm.
[0015] Preferably, in step S4, the rotation speed of the stirring head is 1600-1900 r / min.
[0016] Preferably, in step S4, the welding speed is 500-700 mm / min.
[0017] Preferably, in step S5, the rotation speed of the stirring head is 1400-1600 r / min.
[0018] Preferably, in step S5, the welding speed is 250-350 mm / min.
[0019] Preferably, in step S6, the rotation speed of the stirring head is 1700-1900 r / min.
[0020] Preferably, in step S6, the small magnesium plate pieces are rectangular blocks of 3x4x2 mm.
[0021] Preferably, in step S7: when no obvious defects are found in the X-ray flaw detection results, the actual production and use requirements are met.
[0022] The present invention has the following beneficial effects compared with the prior art:
[0023] The present invention discloses a friction stir welding method for an integrated die-cast magnesium alloy battery case. The overall welding is completed by grinding and cleaning before welding, fixing of tooling fixtures, spot welding fixing, and reasonable design of the welding sequence and welding parameters during welding. The deformation after welding is small and the overall mass of the case is reduced by 1 / 3 compared with that of aluminum alloy. After welding, X-ray flaw detection and three-coordinate detection are carried out, and no obvious defects such as pores, cracks and incomplete penetration are found. In addition, the flash and burr defects are small, and the welding deformation is small, which meets the production requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of a friction stir welding method for an integrated die-cast magnesium alloy battery case.
[0025] Figure 2It is a magnesium alloy profile cover plate exemplified in a stir friction welding method for an integrated die-cast magnesium alloy battery case of the present invention.
[0026] Figure 3 It is a schematic diagram of pre-welding of a battery case as an example in a friction stir welding method for an integrated die-cast magnesium alloy battery case of the present invention.
[0027] Figure 4 It is a schematic diagram of a welding sequence exemplified in a friction stir welding method for an integrated die-cast magnesium alloy battery case of the present invention.
[0028] Figure 5 This is an X-ray flaw detection diagram exemplified in the friction stir welding method of an integrated die-cast magnesium alloy battery case of the present invention.
[0029] Figure 6 This is an X-ray flaw detection diagram exemplified in the friction stir welding method of an integrated die-cast magnesium alloy battery case of the present invention. DETAILED DESCRIPTION
[0030] The following is based on the attached Figure 1-6 The present invention is further described:
[0031] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.
[0033] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0034] like Figure 1As shown, the first embodiment of the present invention provides a friction stir welding method for an integrated die-cast magnesium alloy battery box based on the prior art, and the specific steps are as follows:
[0035] Step S1: Grind the front and back sides of the magnesium alloy profile cover and the weld of the integrated water jacket of the magnesium alloy box with 400#-1000# sandpaper, and clean with alcohol and acetone after grinding;
[0036] Step S2: placing the box body on a special tooling for the friction stir welding machine, placing the cover plate on the welding bead of the box body, and fixing the cover plate and the box body with a clamp;
[0037] Step S3: The clamp is fixed at multiple points on the outermost lap weld. During welding, the multiple-point clamp is lifted up in sequence as the stirring head passes by, and is lowered and clamped after a certain section of the weld is completed.
[0038] Step S4: The flat-head stirring head is first fixed by multi-point welding on the outermost weld bead, the stirring head speed is 1600-1900 r / min, the welding speed is 500-700 mm / min, and pre-welding is performed again for one circle with the same process parameters;
[0039] Step S5: After replacing the pointed stirring head, welding is performed from the outermost circle, the stirring head speed is 1400-1600 r / min, the welding speed is 250-350 mm / min, and then welding is performed according to the designed welding sequence and the same welding process parameters;
[0040] Step S6: Pull out the stirring needle without rotating at the arc end of all welds, replace the flat-head stirring head after welding, and fill the keyhole with a small piece of the same magnesium plate. The filling process parameter is a stirring head speed of 1700-1900r / min;
[0041] Step S7: After cleaning the burrs after welding, perform X-ray flaw detection. If no obvious defects are found in the X-ray flaw detection results, it meets the actual production and use requirements.
[0042] Based on the above-mentioned friction stir welding method, the specific examples are as follows:
[0043] The AZ31 magnesium alloy profile cover with a thickness of 2 mm and a size of Figure 2 As shown in the magnesium alloy box weld, Figure 3 The weld shown is cleaned with 400#~800# sandpaper, and the surface impurities and oil are wiped with alcohol and acetone to remove them. A 2mm thick AZ31 magnesium alloy cover plate is cut into 3x4x2mm rectangular magnesium blocks by wire cutting for keyhole filling;
[0044] Place the box on the special tooling of the friction stir welding machine, place the cover plate on the box weld, fix the cover plate and the outermost weld of the box with a clamp, use a flat head stirring head with a shoulder of 20mm, a stirring head speed of 1800r / min, a welding speed of 600mm / min, and a downward pressure of 2mm. Figure 3 As shown, the outermost circle is spot welded and fixed, and then pre-welded with this parameter for one circle, and then the pointed stirring head is replaced, the stirring needle diameter is 4mm, the shoulder diameter is 20mm, the inclination angle is 2°, the stirring head speed is 1500r / min, the welding speed is 300mm / min, the downward pressure is 3.75mm plus manual fine-tuning. After the outermost circle is welded, this process parameter is still used. Figure 4 The welding sequence shown is 1→13, and the welding is performed from left to right until the box body and the cover plate are welded. The "downward pressure amount" in this embodiment refers to the distance from the shaft shoulder to the welded part;
[0045] After welding, the pointed stirring head was pulled out and replaced with a flat stirring head. A 3x4x2 mm rectangular AZ31 small magnesium block was placed at the keyhole of the weld. The keyhole of each weld was filled in turn at a speed of 1800 r / min until the welding was completed. The flash burrs were cleaned after welding.
[0046] The box body welded joints obtained in this embodiment are subjected to X-ray flaw detection: the X-ray flaw detection results are as follows: Figure 5 and 6 As shown, the weld is well formed, with no obvious defects such as pores, cracks, and incomplete penetration, which meets the requirements of actual production and use.
[0047] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and the embodiments. It can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily realized. Therefore, without departing from the general concept defined by the claims and equivalent scope, the present invention is not limited to the specific details and the illustrations shown and described here.
Claims
1. A friction stir welding method for an integrated die-cast magnesium alloy battery case, characterized in that: include: Step S1, grinding the front and back surfaces of the magnesium alloy profile cover plate and the welds of the magnesium alloy box integrated water jacket with sandpaper, and cleaning with alcohol and acetone after grinding; Step S2, placing the box body on a special tooling for the friction stir welding machine, placing the cover plate on the welding bead of the box body, and fixing the cover plate and the box body with a clamp; Step S3, the clamp is fixed at multiple points on the lap weld of the outermost circle, and during welding, the multiple-point clamp will be lifted up and then lowered to fix and clamp in sequence as the stirring head passes by; Step S4, the flat-head stirring head is first fixed by multi-point welding on the outermost weld bead, and then pre-welded for one circle; Step S5, after replacing the pointed stirring head, welding is performed from the outermost circle, and then welding is performed according to the designed welding sequence and welding process parameters; Step S6, the stirring needle is pulled out without rotation at the arc closing point of all welds, and the flat-head stirring head is replaced after welding, and the keyhole is filled with a small piece of the same magnesium plate; Step S7, after welding, the burrs are cleaned and then X-ray flaw detection is performed.
2. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In the step S1, the sandpaper used is 400#-1000#.
3. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In the step S1: the thickness of the magnesium alloy profile cover plate is 2 mm.
4. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In step S4: the rotation speed of the stirring head is 1600-1900 r / min.
5. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 4, characterized in that: In the step S4: the welding speed is 500-700 mm / min.
6. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In step S5: the rotation speed of the stirring head is 1400-1600 r / min.
7. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 6, characterized in that: In step S5: the welding speed is 250-350 mm / min.
8. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In step S6: the rotation speed of the stirring head is 1700-1900 r / min.
9. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 8, characterized in that: In step S6: the magnesium plate small piece is a cuboid of 3x4x2 mm.
10. The friction stir welding method for an integrated die-cast magnesium alloy battery case according to claim 1, characterized in that: In step S7: when no obvious defects are found in the X-ray flaw detection results, it meets the actual production and use requirements.