Explosive welding process method for bridge and building support

By using explosive welding technology between the stainless steel plates and steel substrates of bridges and building support, the problem of inseparable bonding of argon arc welding is solved, and the combination of solid metallurgy and efficient welding is achieved, which extends the service life of the product.

CN119057486AActive Publication Date: 2024-12-03LUOYANG SUNRUI SPECIAL EQUIP

Patent Information

Application Number
CN202411000084.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-03
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

During the use of traditional bridge support and building support, since the stainless steel plate and steel substrate are sealed and welded by argon arc welding, good bonding cannot be achieved, resulting in hollows and wrinkles in the middle of the stainless steel plate, which affects the use. life.

Method used

The explosive welding process is adopted to ensure that the stainless steel plate and steel substrate are evenly spread explosives between the stainless steel plate and the steel substrate, and ignite the detonator to detonate, forming a high-speed inclined collision zone, achieving a strong metallurgy combination, ensuring the comprehensive bond between the stainless steel plate and the steel substrate.

Benefits of technology

The bonding strength between stainless steel plate and steel substrate is improved, hollowing and wrinkles are avoided, the service life of the product is extended, and the finishing size and surface quality of the parts are ensured through subsequent leveling and polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057486A_ABST
    Figure CN119057486A_ABST
Patent Text Reader

Abstract

The invention discloses an explosive welding process method for a bridge and a building support. The explosive welding process method comprises the following steps that S1, the upper end face of a base plate and the lower end face of a compound plate are polished and cleaned up, and a rusted structure and greasy dirt are removed; s2, the distance between the base plate and the compound plate is controlled according to technological requirements, explosive is evenly laid on the upper surface of the compound plate, a detonator is arranged at one end of the upper end face of the compound plate, and the detonator is inserted into the explosive; s3, implementing explosion: igniting a detonator, and detonating the explosive by the detonator to obtain an explosive composite board; s4, ultrasonic flaw detection is conducted on the explosive composite board, and the internal binding rate is detected; s5, the qualified explosive composite board is leveled; s6, machining is conducted according to a machining drawing and technological requirements; all areas of the compound plate can be comprehensively combined with the base plate, especially the middle part of the compound plate can be tightly attached to the base plate, hollowing and wrinkling cannot be generated, and the service life of subsequent products can be effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bridge and building support welding, and in particular to an explosion welding process method for bridge and building supports. Background Art

[0002] The friction pair of traditional bridge bearings and building bearings is composed of stainless steel plates and polymer materials. The stainless steel plates and the bearing steel base are sealed by argon arc welding. The shape of stainless steel is generally flat or spherical. Figure 1 As shown, the spherical type Figure 2 shown.

[0003] For bridge bearings and building bearings, when the stainless steel plate used in the friction pair is large in size, argon arc welding only on all sides cannot make the stainless steel plate fit well with the steel substrate, especially the middle part of the stainless steel plate is not constrained and fit closely with the steel substrate of the bearing, which is prone to hollowing and wrinkling. During use, the stainless steel plate and the polymer material are constantly rubbed, which will cause the stainless steel plate to expand and deform due to heat over time, and the middle part will bulge, seriously affecting the normal use of bridge bearings and building bearings. Summary of the invention

[0004] The purpose of the present invention is to provide an explosion welding process method for bridge and building supports, aiming to improve the problem that the stainless steel plates of existing bridge supports and building supports are connected to the steel substrate by argon arc welding on all sides. When the stainless steel plates used in the friction pairs are large in size, the stainless steel plates and the steel substrate cannot be well fitted, resulting in hollowing and wrinkles, which in turn causes the stainless steel plates to expand and deform due to heat under long-term use, seriously affecting the normal use of bridge supports and building supports.

[0005] In order to achieve the above object, the present invention provides an explosion welding process for bridges and building supports, comprising the following steps:

[0006] S1. Grind and clean the upper end surface of the base plate and the lower end surface of the composite plate to remove rust and oil stains;

[0007] S2. Control the distance between the base plate and the double plate according to the process requirements, evenly spread the explosives on the upper surface of the double plate, and arrange a detonator at one end of the upper end surface of the double plate, wherein the detonator is inserted into the explosives;

[0008] S3, carrying out explosion: igniting the detonator, the detonator detonates the explosive, and obtains the explosive composite plate;

[0009] S4. Perform ultrasonic flaw detection on the explosive composite plate to detect the internal bonding rate;

[0010] S5. Level the qualified explosive composite panels;

[0011] S6. Carry out machining according to machining drawings and process requirements.

[0012] Furthermore, the method further comprises the following steps:

[0013] S0. Conduct chemical composition, mechanical property inspection and dimensional re-inspection on the base plate and the composite plate, and conduct ultrasonic flaw detection when necessary to ensure that the performance of the raw materials meets the technical requirements and eliminate unqualified base plates and composite plates.

[0014] Furthermore, the method further comprises the following steps:

[0015] S7. Polish the surface of the composite board with sandpapers of 80 mesh, 200 mesh, 400 mesh and 800 mesh respectively. After polishing, clean the surface of the composite board. After cleaning, apply a layer of water-oil dual-soluble diamond grinding paste on the surface of the composite board and grind it to achieve a mirror effect.

[0016] Furthermore, in step S4, a spreading tool is used to spread the explosives on the upper surface of the composite plate, so that the thickness of the explosives at various locations on the upper surface of the composite plate is uniform and meets the process requirements.

[0017] Furthermore, the paving tool comprises a paving cylinder, the paving cylinder is connected to a paving rod, and both ends of the paving cylinder are rotatably connected to a roller, and the roller is in the shape of a thin sheet.

[0018] Furthermore, an n-shaped frame is provided on the outer cylindrical wall of the paving cylinder, the paving rod is connected to the middle part of the transverse part of the n-shaped frame, and the paving rod is aligned with the middle position of the paving cylinder.

[0019] Furthermore, a connecting shaft is rotatably connected to the middle of the roller, and both ends of the paving cylinder are detachably connected to the two connecting shafts, and the paving cylinder and the connecting shafts have a common central axis.

[0020] Furthermore, a connecting hole is provided at the end of the connecting shaft near the paving cylinder, and the connecting hole is a cylindrical hole, and the connecting hole and the connecting shaft have a central axis; a threaded through hole leading to the connecting hole is provided on the connecting shaft, and a fixing bolt is installed in the threaded through hole; an intermediate shaft is provided at each end of the paving cylinder, and a plug-in shaft is provided at the end of the intermediate shaft, and the plug-in shaft and the intermediate shaft are both coaxial with the paving cylinder, and the diameter of the plug-in shaft is the same as the aperture of the connecting hole; when the connecting shaft and the paving cylinder are connected to each other, the plug-in shafts at both ends of the paving cylinder are respectively inserted into the connecting holes of the two connecting shafts and are fixed by two fixing bolts.

[0021] Furthermore, the outer end of the roller is evenly provided with a plurality of cutting openings along its circumferential direction, wherein the cutting openings include a connecting cutting portion and a circular hole portion, wherein the width of the cutting portion is smaller than the aperture of the circular hole portion, and the cutting portion smoothly transitions to the circular hole portion.

[0022] Furthermore, the central angle of the cut corresponding to the cut is θ, then θ satisfies the formula: θ≤2×arccos(1-L / R), wherein L is the maximum allowable difference in the thickness of the explosive at various locations, and R is the radius of the roller.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention is driven by the energy generated by the explosion of explosives, so that the upper surface of the substrate and the lower surface of the composite plate collide at a high speed, forming a thin layer of composite transition zone with plastic deformation, melting, diffusion and waveform characteristics on the metal interface to be bonded, forming a strong metallurgical bond with the advantage of high welding strength.

[0025] 2. The present invention can make large-sized support plates be explosively composited in one step through explosive welding, which has the advantage of high welding efficiency.

[0026] 3. The present invention can make all areas of the composite board fully combined with the substrate, especially the middle part of the composite board can be closely attached to the substrate without hollowing and wrinkling, which can effectively improve the service life of subsequent products.

[0027] 4. After the explosion is completed, the present invention can ensure the fine processing size and surface quality of the parts through leveling, machining, surface grinding and polishing.

[0028] 5. The present invention spreads the explosives by means of a spreading tool, so that the thickness of the explosives at various locations on the upper surface of the composite plate can be uniform, meeting the process requirements and providing an effective guarantee for the effect of explosive welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the planar welding structure of the existing stainless steel plate and the support steel matrix;

[0030] Figure 2 It is a schematic diagram of the spherical welding structure of the existing stainless steel plate and the support steel matrix;

[0031] Figure 3 is a schematic diagram of the explosion arrangement of the present invention;

[0032] Figure 4 It is a schematic diagram of the explosion welding process of the present invention;

[0033] Figure 5 is a schematic diagram of the three-dimensional structure of the paving tool used in the present invention;

[0034] Figure 6 It is a three-dimensional structural schematic diagram of the roller and the connecting shaft of the paving tool used in the present invention;

[0035] Figure 7It is a schematic diagram of the three-dimensional structure of the roller of the paving tool used in the present invention.

[0036] Figure numerals: 1, base plate; 2, double plate; 3, explosive; 4, detonator; 6, paving cylinder; 601, intermediate shaft; 7, paving rod; 8, roller; 801, cutting mouth; 9, connecting shaft; 901, connecting hole; 10, N-shaped frame; 11, fixing bolt. DETAILED DESCRIPTION

[0037] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0038] The following is a further description with reference to the accompanying drawings and specific embodiments:

[0039] An explosive welding process for bridge and building supports comprises the following steps:

[0040] S0. Test the chemical composition, mechanical properties and dimensions of the base plate 1 and the composite plate 2, and perform ultrasonic flaw detection if necessary to ensure that the raw material properties meet the technical requirements, and remove unqualified base plates 1 and composite plates 2. The base plate 1 is a support steel base material, and the composite plate 2 uses a stainless steel plate.

[0041] S1. Grind and clean the upper end surface of the base plate 1 and the lower end surface of the composite plate 2 to remove rusted structures and oil stains.

[0042] S2, such as Figure 3 As shown, the distance T between the base plate 1 and the composite plate 2 is controlled according to the process requirements, the explosive 3 is evenly spread on the upper surface of the composite plate 2, and the detonator 4 is arranged at one end of the upper end surface of the composite plate 2, and the detonator 4 is inserted into the explosive 3.

[0043] S3, carry out explosion: ignite the detonator 4, the detonator 4 detonates the explosive 3, and obtains the explosive composite plate. The explosive welding process is as follows Figure 4 shown.

[0044] S4. Perform ultrasonic flaw detection on the explosive composite panels to detect the internal bonding rate, and eliminate the explosive composite panels with unqualified internal bonding rates.

[0045] S5. Level the qualified explosive composite panels.

[0046] S6. Carry out machining according to machining drawings and process requirements.

[0047] S7. Polish the surface of the composite plate 2 with sandpapers of 80 mesh, 200 mesh, 400 mesh and 800 mesh respectively. After polishing, clean the surface of the composite plate 2. After cleaning, apply a layer of water-oil dual-soluble diamond grinding paste on the surface of the composite plate 2 and grind it to achieve a mirror effect.

[0048] The process principle of the present invention is: when performing explosion welding, according to Figure 3 As shown, the substrate 1, the composite plate 2 and the explosive 3 are arranged, and a buffer layer can also be set between the composite plate 2 and the explosive 3. After the arrangement is completed, explosive welding is carried out, and the detonator 4 is ignited. The detonator 4 detonates the explosive 3, and the energy generated by the explosion of the explosive 3 is used to drive the upper surface of the substrate 1 and the lower surface of the composite plate 2 to collide with each other at a high speed, and a thin layer of composite transition zone with plastic deformation, melting, diffusion and waveform characteristics is formed on the metal interface to be combined, forming a strong metallurgical bond with the advantage of high welding strength. Moreover, through explosive welding, large-sized support plates can be explosively composited at one time, which has the advantage of high welding efficiency. All areas of the composite plate 2 can be fully combined with the substrate 1, especially the middle part of the composite plate 2 can be closely attached to the substrate 1, and no hollowing and wrinkles will be generated, which can effectively improve the service life of subsequent products.

[0049] like Figure 5 and Figure 6 As shown, in step S4, a paving tool is used to spread the explosive 3 on the upper surface of the double plate 2, so that the thickness of the explosive at various locations on the upper surface of the double plate 2 is uniform, meeting the process requirements. The paving tool includes a paving cylinder 6 and two rollers 8, an n-shaped frame 10 is provided on the outer cylindrical wall of the paving cylinder 6, and a paving rod 7 is connected to the middle part of the transverse part of the n-shaped frame 10, and the paving rod 7 is aligned with the middle position of the paving cylinder 6. The two ends of the paving cylinder 6 are respectively connected to the two rollers 8 for rotation, so that the rollers 8 can be pushed by the paving rod 7 to drive the paving cylinder 6 to evenly spread the explosive 3 on the upper surface of the double plate 2, so that the thickness of the explosive at various locations on the upper surface of the double plate 2 is uniform, meeting the process requirements.

[0050] like Figure 5 and Figure 6As shown, the middle part of the roller 8 is rotatably connected with a connecting shaft 9, and the two ends of the paving cylinder 6 are detachably connected to the two connecting shafts 9, and the paving cylinder 6 and the connecting shafts 9 share the same center axis. The connecting shaft 9 is provided with a connecting hole 901 at the end close to the paving cylinder 6. The connecting hole 901 is a cylindrical hole, and the connecting hole 901 and the connecting shaft 9 share the same center axis; the connecting shaft 9 is provided with a threaded through hole leading to the connecting hole 901, and a fixing bolt 11 is installed in the threaded through hole. An intermediate shaft 601 is provided at each end of the paving cylinder 6, and a plug-in shaft is provided at the end of the intermediate shaft 601. The plug-in shaft and the intermediate shaft 601 are both shared with the paving cylinder 6. The diameter of the plug-in shaft is the same as the aperture of the connecting hole 901. When the connecting shaft 9 is connected to the paving cylinder 6, the plug-in shafts at both ends of the paving cylinder 6 are respectively inserted into the connecting holes 901 of the two connecting shafts 9 and fixed by two fixing bolts 11. In this way, according to different process requirements, the paving cylinder 6 with different outer diameters can be replaced and used, so that the thickness of the explosive 3 after being spread by the paving cylinder 6 meets the corresponding process requirements.

[0051] To achieve uniform thickness of explosives at various locations on the upper surface of the double plate 2, the roller 8 is required to be able to directly contact the upper surface of the double plate 2, so the roller 8 is set to be in the shape of a thin sheet, such as Figure 7 As shown, the roller 8 is convenient to pass through the explosive 3 and directly contact the upper surface of the double plate 2. The outer end of the roller 8 is evenly provided with a plurality of cutting openings 801 along its circumferential direction. The cutting opening 801 includes a connected cutting portion and a circular hole portion. The width of the cutting portion is smaller than the aperture of the circular hole portion, and the cutting portion smoothly transitions to the circular hole portion. The cutting portion is used to cut the explosive layer. The explosive at the cutting position enters the circular hole portion with a large aperture, which helps to reduce the cutting resistance. In this way, the roller 8 has a strong cutting ability, so that when the thickness of the explosive 3 is large, the roller 8 can still pass through the explosive 3 and directly contact the upper surface of the double plate 2, effectively ensuring that the explosive 3 is spread evenly and meeting the process requirements. The central angle corresponding to the cutting position of the cutting opening 801 is θ, and θ satisfies the formula: θ≤2×arccos(1-L / R), where L is the maximum difference allowed for the paving thickness of the explosive 3 at each location, and R is the radius of the roller 8. The above arrangement ensures that when the above-mentioned paving tool is used to spread the explosive 3, the roller 8 has a strong cutting ability so that the roller 8 can pass through the explosive 3 and directly contact the upper surface of the composite plate 2, and the difference in the paving thickness of the explosive 3 at various locations is less than or equal to the maximum allowed difference.

[0052] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An explosive welding process for bridge and building supports, It is characterized in that The steps include: S1. Grind and clean the upper end surface of the base plate (1) and the lower end surface of the composite plate (2) to remove rust and oil stains; S2. Control the distance between the base plate (1) and the composite plate (2) according to the process requirements, evenly spread the explosive (3) on the upper surface of the composite plate (2), and arrange a detonator (4) at one end of the upper end surface of the composite plate (2), wherein the detonator (4) is inserted into the explosive (3); S3, carrying out explosion: igniting the detonator (4), the detonator (4) detonates the explosive (3), and obtains the explosive composite plate; S4. Perform ultrasonic flaw detection on the explosive composite plate to detect the internal bonding rate; S5. Level the qualified explosive composite panels; S6. Carry out machining according to machining drawings and process requirements.

2. The explosive welding process for bridges and building supports according to claim 1, It is characterized in that The following steps are also included: S0. The base plate (1) and the composite plate (2) are tested for chemical composition, mechanical properties and dimensions, and ultrasonic flaw detection is performed when necessary to ensure that the properties of the raw materials meet the technical requirements, and unqualified base plates (1) and composite plates (2) are discarded.

3. The explosive welding process for bridges and building supports according to claim 1, It is characterized in that The following steps are also included: S7. The surface of the composite plate (2) is polished with sandpapers of 80 mesh, 200 mesh, 400 mesh and 800 mesh, respectively. After polishing, the surface of the composite plate (2) is cleaned. After cleaning, a layer of water-oil dual-soluble diamond grinding paste is applied on the surface of the composite plate (2), and then polished to achieve a mirror effect.

4. The explosive welding process for bridge and building supports according to claim 1, It is characterized in that In the step S4, a spreading tool is used to spread the explosive (3) on the upper surface of the composite plate (2), so that the thickness of the explosive at various locations on the upper surface of the composite plate (2) is uniform and meets the process requirements.

5. The explosive welding process for bridge and building supports according to claim 4, It is characterized in that The paving tool comprises a paving cylinder (6), the paving cylinder (6) is connected to a paving rod (7), and both ends of the paving cylinder (6) are rotatably connected to a roller (8), and the roller (8) is in the shape of a thin sheet.

6. The explosive welding process for bridge and building supports according to claim 5, It is characterized in that An n-shaped frame (10) is arranged on the outer cylindrical wall of the paving cylinder (6), the paving rod (7) is connected to the middle part of the transverse part of the n-shaped frame (10), and the paving rod (7) is aligned with the middle position of the paving cylinder (6).

7. The explosive welding process for bridge and building supports according to claim 5, It is characterized in that The middle part of the roller (8) is rotatably connected to a connecting shaft (9), and the two ends of the paving cylinder (6) are detachably connected to the two connecting shafts (9), and the paving cylinder (6) and the connecting shaft (9) share a common central axis.

8. The explosive welding process for bridge and building supports according to claim 7, It is characterized in that The connecting shaft (9) is provided with a connecting hole (901) at the end near the paving cylinder (6); the connecting hole (901) is a cylindrical hole, and the connecting hole (901) and the connecting shaft (9) are coaxial; the connecting shaft (9) is provided with a threaded through hole leading to the connecting hole (901), and a fixing bolt (11) is installed in the threaded through hole; an intermediate shaft (601) is provided at each end of the paving cylinder (6), and a plug-in shaft is provided at the end of the intermediate shaft (601), and the plug-in shaft and the intermediate shaft (601) are coaxial with the paving cylinder (6), and the diameter of the plug-in shaft is the same as the hole diameter of the connecting hole (901); when the connecting shaft (9) and the paving cylinder (6) are connected, the plug-in shafts at both ends of the paving cylinder (6) are respectively inserted into the connecting holes (901) of the two connecting shafts (9) and are fixed by two fixing bolts (11).

9. The explosive welding process for bridge and building supports according to claim 5, It is characterized in that The outer end of the roller (8) is evenly provided with a plurality of cutting openings (801) along its circumferential direction, the cutting openings (801) comprising a connecting cutting portion and a circular hole portion, the width of the cutting portion being smaller than the aperture of the circular hole portion, and the cutting portion smoothly transitions to the circular hole portion.

10. The explosive welding process for bridge and building supports according to claim 9, It is characterized in that The central angle of the cutout (801) is θ, and θ satisfies the formula: θ≤2×arccos(1-L / R), wherein L is the maximum difference allowed for the paving thickness of the explosive (3) at various locations, and R is the radius of the roller (8).

Citation Information

Patent Citations

  • Explosive welding method of 317L austenitic stainless steel clad steel plate

    CN101559520A

  • Explosive welding method of SAF2507 alloy composite steel plate

    CN101837511A

  • Explosive pushing cart for explosive welding and arrangement

    CN104741767A

  • Explosive bulldozing mechanism for explosive welding of composite board

    CN218745508U

  • Process for plating guide rails in machine tools and similar structural parts with sliding materials using an explosive

    DE1752926A1

Cited By

  • Explosive welding method for composite spherical crown lining plate

    CN119681405A