Method for extracting iron and aluminum in wet-process phosphoric acid step by step

By adjusting the volume ratio of the extractant and using specific extractant, iron and aluminum ions in wet phosphoric acid are extracted step by step, the problem of difficult separation in the prior art is solved, efficient separation and selective recycling are achieved, and product quality is improved and industrial applicability.

CN119059499AActive Publication Date: 2024-12-03INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411491626.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03
Estimated Expiration
2044-10-24

Smart Images

  • Figure CN119059499A_ABST
    Figure CN119059499A_ABST
Patent Text Reader

Abstract

The invention relates to a method for extracting iron and aluminum in wet-process phosphoric acid step by step, which comprises the following steps: mixing a first extraction system and wet-process phosphoric acid according to a volume ratio of 1: (1-6), and carrying out first extraction to obtain iron-removed phosphoric acid; mixing a second extraction system with the iron-removed phosphoric acid obtained in the step (1) according to a volume ratio of (1.2-6): 1, and carrying out second extraction to obtain iron-removed and aluminum-removed phosphoric acid; the first extraction system and the second extraction system respectively and independently comprise an extraction agent containing phosphorus-oxygen double bonds and / or an extraction agent containing phosphorus hydroxyl; according to the method, iron and aluminum in wet-process phosphoric acid are extracted step by step, the extraction rate of iron ions can reach 99% or above, and the extraction rate of aluminum ions can reach 88% or above; the resource utilization value of the industrial wet-process phosphoric acid is improved, the technological process is short, the raw material cost is low, and industrialization is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of resource and environmental technology, and in particular to a method for extracting iron and aluminum in wet-process phosphoric acid in steps. Background Art

[0002] Phosphoric acid is an important product in the phosphorus chemical industry and an important chemical raw material in industrial production. It can be used to prepare chemical fertilizers, detergents, food and feed additives, etc. The wet process phosphoric acid has become the mainstream process for preparing phosphoric acid from phosphate rock due to its advantages such as low cost and low energy consumption. However, wet process phosphoric acid often contains a variety of impurities, such as metal ions such as iron ions and aluminum ions. These impurities not only affect product quality and hinder the back-end application of the product, but also damage production equipment and the environment. Therefore, it is very important to analyze and treat the impurities in wet process phosphoric acid.

[0003] At present, the main methods for purifying wet-process phosphoric acid in industry include crystallization, ion exchange, solvent precipitation, organic solvent extraction, concentration purification, and electrodialysis. The solvent extraction method for purifying wet-process phosphoric acid has become the mainstream method for purifying and removing impurities from wet-process phosphoric acid due to its advantages of good separation effect, low raw material consumption, and low impurity removal energy consumption. A large number of studies have been conducted on impurity removal of wet-process phosphoric acid, but all of them are aimed at achieving efficient separation and selective recycling of iron ions and aluminum ions with very similar chemical properties as impurity ions in wet-process phosphoric acid.

[0004] For example, CN110116997A discloses a method for purifying and removing iron from wet-process phosphoric acid. In this method, divalent ferrous ions in crude phosphoric acid are first oxidized to trivalent ferrous ions using hydrogen peroxide, and then tributyl phosphate and kerosene are used for multi-stage extraction and stripping to achieve the removal of impure iron ions. This method has a complex extraction process and high equipment requirements, and does not further remove aluminum ions with similar chemical properties to iron ions, and does not achieve efficient separation and recycling of impure aluminum ions in wet-process phosphoric acid.

[0005] CN101920946B discloses a method for reducing iron and aluminum ions in wet-process phosphoric acid. The method comprises firstly subjecting the wet-process phosphoric acid to oxidation treatment with hydrogen peroxide, and then adding potassium oxalate and sodium carbonate to the oxidized wet-process phosphoric acid for chemical reaction treatment, thereby partially removing the iron and aluminum ions in the wet-process phosphoric acid. The method simultaneously removes part of the iron and aluminum ions in the wet-process phosphoric acid, and does not achieve efficient separation and recycling of iron and aluminum ions, and the maximum removal rate of iron ions is only 70%.

[0006] Therefore, how to achieve efficient separation of iron ions and aluminum ions with similar chemical properties in wet-process phosphoric acid for selective and separate recovery has become a problem that needs to be solved urgently. Summary of the invention

[0007] In order to solve the above technical problems, the method of the present invention first extracts iron in wet-process phosphoric acid at a lower O / A ratio, then adjusts the O / A ratio, and further extracts aluminum at a larger O / A ratio, so that iron and aluminum in wet-process phosphoric acid can be extracted step by step, and then the efficient separation and selective recovery of iron and aluminum in wet-process phosphoric acid are achieved, thereby improving the comprehensive utilization of wet-process phosphoric acid, and having the advantages of simple process flow, low cost, no secondary pollution, and easy industrialization.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps, the method comprising the following steps:

[0010] (1) mixing the first extraction system and wet-process phosphoric acid in a volume ratio of 1:(1-6) to perform a first extraction to obtain iron-removing phosphoric acid;

[0011] (2) mixing the second extraction system and the iron-removing phosphoric acid described in step (1) at a volume ratio of (1.2-6):1 to perform a second extraction to obtain the iron-removing aluminum phosphoric acid;

[0012] Wherein, the first extraction system and the second extraction system each independently comprise an extractant containing a phosphorus-oxygen double bond and / or an extractant containing a phosphorus hydroxyl group.

[0013] Wherein, in step (1), the volume ratio of the first extraction system to the wet-process phosphoric acid is 1:(1-6), for example, it can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6, etc.

[0014] The volume ratio of the second extraction system in step (2) to the iron-removing phosphoric acid in step (1) is (1.2-6):1, for example, it can be 1.2:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1 or 6:1, etc.

[0015] The invention extracts iron and aluminum in wet-process phosphoric acid in steps by adjusting the O / A ratio. The iron ions in the wet-process phosphoric acid are firstly extracted at an O / A ratio of 1:(1-6) to obtain iron-free phosphoric acid, and then the aluminum ions in the iron-free phosphoric acid are extracted at an O / A ratio of (1.2-6):1 to obtain iron-free aluminum phosphoric acid. The technical problem that iron ions and aluminum ions with similar properties in the wet-process phosphoric acid are difficult to separate and separately recover is solved, and the foundation is laid for the subsequent high-quality utilization of iron-free aluminum phosphoric acid. The method has a simple process flow, low cost and is easy to industrialize.

[0016] It is worth noting that when the first extraction system and the second extraction system in the present invention extract iron ions and aluminum ions, there is a competition mechanism between the two ions. Iron ions have an advantage in the competition due to their stronger complexing ability. The extraction system is more inclined to react chemically with iron ions to form a stable complex, while the extraction of aluminum ions is relatively weak. This selectivity determines that under the same O / A ratio conditions, the extraction rate of iron is higher, and a higher extraction efficiency can be achieved at a lower O / A ratio.

[0017] The present invention selects the first extraction system and the second extraction system to independently include an extractant containing a phosphorus-oxygen double bond and / or an extractant containing a phosphorus-hydroxyl group, and utilizes the phosphorus-oxygen double bond and the phosphorus-hydroxyl bond in the extractant to coordinate with the iron ion and the aluminum ion and form a stable complex. Due to the presence of the phosphorus-oxygen double bond, the extractant has a certain acidity, and this acidity enables the extractant to exchange with the metal cations (such as iron ions and aluminum ions) in the aqueous phase. The stronger the acidity, the greater the ability to extract the iron ions and aluminum ions. In addition, the oxygen atom in the phosphorus-oxygen double bond has a strong electrophilicity and can attract metal cations to form a stable complex, thereby achieving extraction; the hydrogen ions in the phosphorus-hydroxyl bond can form hydrogen bonds with water molecules or other oxygen-containing groups, which helps the extractant to disperse in the aqueous phase and contact with the iron ions and aluminum ions. At the same time, the hydrogen ions exchange with the anions in the aqueous phase, so that the iron ions and aluminum ions are transferred from the aqueous phase to the organic phase, achieving extraction and separation.

[0018] It is worth emphasizing that the first extraction system and the second extraction system of the present invention may be the same or different, and each is independently selected from an extractant containing a phosphorus-oxygen double bond and / or an extractant containing a phosphorus hydroxyl group.

[0019] Preferably, in step (1), the volume ratio of the first extraction system to wet-process phosphoric acid is 1:(1-3).

[0020] Preferably, the volume ratio of the second extraction system in step (2) to the iron-removing phosphoric acid in step (1) is (4-6):1.

[0021] It is worth noting that the present invention further preferably has a volume ratio of the first extraction system to the wet-process phosphoric acid of 1:(1-3), and a volume ratio of the second extraction system to the phosphoric acid for removing iron in step (1) of step (2) of (4-6):1, which further improves the efficient and selective step-by-step extraction of iron ions and aluminum ions in the wet-process phosphoric acid; if the volume ratio of the first extraction system to the wet-process phosphoric acid of step (1) is too low, the extraction cost will increase and the iron ion extraction distribution ratio will decrease; if the volume ratio of the first extraction system to the wet-process phosphoric acid of step (1) is too high, the iron ions and aluminum ions in the wet-process phosphoric acid will be extracted at the same time, resulting in the subsequent inability to achieve separate recovery of iron ions and aluminum ions; if the volume ratio of the second extraction system to the phosphoric acid for removing iron in step (2) of step (1) is too low, the aluminum ions in the phosphoric acid for removing iron are not fully extracted, resulting in a decrease in the extraction rate of aluminum ions; if the volume ratio of the second extraction system to the phosphoric acid for removing iron in step (1) of step (2) is too high, the extraction rate of aluminum ions is not significantly improved.

[0022] Preferably, the content of iron ions in the wet-process phosphoric acid in step (1) is 0.10-0.50wt% in terms of mass percentage, for example, it can be 0.10wt%, 0.15wt%, 0.20wt%, 0.25wt%, 0.30wt%, 0.35wt%, 0.40wt%, 0.45wt% or 0.50wt%, etc.

[0023] Preferably, the content of aluminum ions in the wet-process phosphoric acid in step (1) is 0.60-3.0 wt%, calculated as a percentage by mass, for example, 0.60 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 2.5 wt% or 3.0 wt%, etc.

[0024] Preferably, the extractant containing phosphorus-oxygen double bonds comprises any one of trialkylphosphine oxide, tributyl phosphate, Cyanex 272, dimethylheptyl methylphosphonate or 2-ethylhexyl diphenyl phosphate, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of trialkylphosphine oxide and tributyl phosphate, a combination of trialkylphosphine oxide and dimethylheptyl methylphosphonate, or a combination of Cyanex 272 and 2-ethylhexyl diphenyl phosphoric acid, and the like.

[0025] Preferably, the phosphorus hydroxyl-containing extractant comprises di(2-ethylhexyl) phosphate and / or 2-ethylhexyl phosphate 2-ethylhexyl ester. Preferably, the first extraction system in step (1) further comprises a first diluent.

[0026] Preferably, the volume ratio of the extractant to the first diluent in the first extraction system is 1:(1-4), for example, it can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 or 1:4, etc., preferably 1:(1-2).

[0027] Preferably, the second extraction system in step (2) further includes a second diluent.

[0028] Preferably, the volume ratio of the extractant to the second diluent in the second extraction system is 1:(1-4), for example, it can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 or 1:4, etc.

[0029] Preferably, the first diluent and the second diluent each independently include any one or a combination of at least two of kerosene, sulfonated kerosene, cyclohexane, xylene, n-heptane or ethyl acetate, wherein typical but non-limiting combinations include a combination of sulfonated kerosene and cyclohexane, a combination of kerosene and cyclohexane, or a combination of sulfonated kerosene and ethyl acetate.

[0030] Preferably, the temperature of the first extraction in step (1) is 20-50°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C.

[0031] Preferably, the first extraction time in step (1) is 5 to 30 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min or 30 min.

[0032] Preferably, the first extraction in step (1) is accompanied by a first stirring.

[0033] Preferably, the first stirring rate is 50-200 r / min, for example, 50 r / min, 80 r / min, 100 r / min, 120 r / min, 150 r / min, 180 r / min or 200 r / min, etc., preferably 100-180 r / min.

[0034] Preferably, the temperature of the second extraction in step (2) is 20-90°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, etc., preferably 60-90°C.

[0035] The present invention further prefers that the temperature of the second extraction is 60-90° C., which is beneficial to the extraction of aluminum ions in the iron-free phosphate; if the temperature of the second extraction is too low, the aluminum ion extraction rate will decrease; if the temperature of the second extraction is too high, the extraction effect will not be significantly improved, but will cause higher energy consumption.

[0036] Preferably, the time of the second extraction in step (2) is 5 to 60 min, for example, 5 min, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0037] Preferably, the second extraction process in step (2) is accompanied by a second stirring.

[0038] Preferably, the second stirring rate is 50-300 r / min, for example, 50 r / min, 100 r / min, 150 r / min, 200 r / min, 250 r / min or 300 r / min, etc., preferably 200-300 r / min.

[0039] The present invention further preferably has a second stirring rate of 200-300 r / min during the second extraction process, which is conducive to sufficient mixing of the second extraction system with the iron-removing phosphoric acid to improve the extraction effect of aluminum ions.

[0040] Preferably, the first extraction and the second extraction methods each independently include single-stage extraction and / or multi-stage extraction; preferably, the first extraction method is single-stage extraction; preferably, the second extraction method is multi-stage extraction.

[0041] Preferably, the extraction stages of the multi-stage extraction are 2 to 5, for example, 2, 3, 4 or 5 stages.

[0042] The present invention further preferably comprises that the first extraction is a single-stage extraction, the second extraction is a multi-stage extraction, and the number of extraction stages is 2 to 5; this not only achieves efficient extraction of iron ions and aluminum ions in wet-process phosphoric acid, but also ensures lower extraction energy consumption.

[0043] Preferably, after the first extraction in step (1), an iron-loaded extractant is obtained.

[0044] Preferably, after the second extraction in step (2), an extractant loaded with aluminum is obtained.

[0045] As a further preferred technical solution of the present invention, refer to Figure 1 The process flow shown in the figure comprises the following steps:

[0046] (1) mixing the first extraction system and wet-process phosphoric acid at a volume ratio of 1:(1-6), performing a first extraction for 5-30 minutes at 20-50° C. and a first stirring rate of 50-200 r / min to obtain iron-removing phosphoric acid and an iron-loaded extractant;

[0047] (2) mixing the second extraction system with the iron-removing phosphoric acid in step (1) at a volume ratio of (1.2-6):1, performing a second extraction for 5-60 minutes at 20-90° C. and a second stirring rate of 50-300 r / min to obtain iron-removing aluminum phosphoric acid; wherein the content of iron ions in the wet-process phosphoric acid in step (1) is 0.10-0.50wt%, and the content of aluminum ions is 0.60-3.0wt%; the first extraction and the second extraction each independently include single-stage extraction and / or multi-stage extraction, and the number of stages of the multi-stage extraction is 2-5;

[0048] The first extraction system and the second extraction system each independently include an extractant containing a phosphorus-oxygen double bond and / or an extractant containing a phosphorus hydroxyl group; the first extraction system also includes a first diluent; the volume ratio of the extractant to the first diluent in the first extraction system is 1:(1-4); the second extraction system also includes a second diluent; the volume ratio of the extractant to the second diluent in the second extraction system is 1:(1-4).

[0049] Optionally, the iron-loaded extractant in step (1) and the aluminum-loaded extractant in step (2) are subjected to stripping, separation and purification steps to further prepare an iron product or an aluminum product; the iron-removed aluminum phosphate is further purified to prepare a phosphorus product.

[0050] Compared with the prior art, the present invention has at least the following beneficial effects:

[0051] (1) The method for extracting iron and aluminum in wet-process phosphoric acid in steps provided by the present invention selects specific O / A ratios respectively to efficiently extract iron ions and aluminum ions in the wet-process phosphoric acid in steps, so as to subsequently separately recover iron ions and aluminum ions in the wet-process phosphoric acid and utilize the wet-process phosphoric acid in high quality. The method has a simple process flow, low cost and is easy to industrialize.

[0052] (2) The method for extracting iron and aluminum in wet-process phosphoric acid in steps provided by the present invention further improves the extraction rate of iron ions and aluminum ions in wet-process phosphoric acid by further optimizing the process parameters such as the O / A ratio, extraction temperature, extraction time, extraction stage, and stirring rate of the first extraction and the second extraction. The extraction rate of iron ions can be as high as more than 99%, and the extraction rate of aluminum ions can be as high as more than 88%. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The present invention provides a process flow chart of the method for extracting iron and aluminum from wet-process phosphoric acid in steps. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described below by specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0055] The wet-process phosphoric acid used in the following examples and comparative examples is from Yichang Xingfa Chemical Co., Ltd., and includes the components shown in Table 1 and the balance water;

[0056] Table 1

[0057] Components Fe Al Mg Si <![CDATA[P2O5]]> Content / wt% 0.205 0.838 0.644 0.118 35.573

[0058] 1. Implementation

[0059] Example 1

[0060] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps, the method comprising the following steps:

[0061] (1) mixing a first extraction system and wet-process phosphoric acid at a volume ratio of 1:1, performing a first extraction for 25 minutes at 30° C. and a first stirring rate of 150 r / min to obtain iron-removing phosphoric acid and an iron-loaded extractant; the first extraction is a single-stage extraction;

[0062] (2) mixing the second extraction system with the iron-removing phosphoric acid described in step (1) at a volume ratio of 5:1, performing a second extraction for 50 minutes at 70° C. and a second stirring rate of 250 r / min to obtain an iron-removing aluminum phosphoric acid and an aluminum-loaded extractant; the second extraction is a multi-stage extraction with 5 extraction stages;

[0063] Wherein, the first extraction system is composed of a dimethylheptyl methylphosphonate extractant and a sulfonated kerosene diluent in a volume ratio of 1:1;

[0064] The second extraction system is consistent with the first extraction system.

[0065] Example 2

[0066] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps, the method comprising the following steps:

[0067] (1) mixing the first extraction system and wet-process phosphoric acid at a volume ratio of 1:1.5, performing a first extraction for 25 minutes at 30° C. and a first stirring rate of 150 r / min to obtain iron-removing phosphoric acid and an iron-loaded extractant; the first extraction is a single-stage extraction;

[0068] (2) mixing the second extraction system with the iron-removing phosphoric acid described in step (1) at a volume ratio of 5:1, performing a second extraction for 50 minutes at 70° C. and a second stirring rate of 250 r / min to obtain an iron-removing aluminum phosphoric acid and an aluminum-loaded extractant; the second extraction is a multi-stage extraction with 5 extraction stages;

[0069] Wherein, the first extraction system is composed of a dimethylheptyl methylphosphonate extractant and a sulfonated kerosene diluent in a volume ratio of 1:1;

[0070] The second extraction system is consistent with the first extraction system.

[0071] Example 3

[0072] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps, the method comprising the following steps:

[0073] (1) mixing a first extraction system and wet-process phosphoric acid at a volume ratio of 1:3, performing a first extraction for 20 minutes at 20° C. and a first stirring rate of 180 r / min to obtain iron-removing phosphoric acid and an iron-loaded extractant; the first extraction is a single-stage extraction;

[0074] (2) mixing the second extraction system with the iron-removing phosphoric acid described in step (1) at a volume ratio of 4:1, performing a second extraction for 40 minutes at 90° C. and a second stirring rate of 200 r / min to obtain an iron-removing aluminum phosphoric acid and an aluminum-loaded extractant; the second extraction is a multi-stage extraction with 5 extraction stages;

[0075] Wherein, the first extraction system is composed of 2-ethylhexyl diphenyl phosphate extractant and sulfonated kerosene diluent in a volume ratio of 1:1.5;

[0076] The second extraction system is consistent with the first extraction system.

[0077] Example 4

[0078] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that in step (1), the volume ratio of the first extraction system to the wet-process phosphoric acid is 1:0.5.

[0079] Example 5

[0080] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that in step (1), the volume ratio of the first extraction system to the wet-process phosphoric acid is 1:3.5.

[0081] Example 6

[0082] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that the volume ratio of the second extraction system in step (2) to the phosphoric acid for removing iron in step (1) is 3.5:1.

[0083] Example 7

[0084] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that the volume ratio of the second extraction system in step (2) to the phosphoric acid for removing iron in step (1) is 6.5:1.

[0085] Example 8

[0086] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Example 1 except that the volume ratio of dimethylheptyl methylphosphonate extractant and sulfonated kerosene diluent in the first extraction system is 1:2.

[0087] Example 9

[0088] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that the second stirring rate in the second extraction process is 180 r / min.

[0089] Example 10

[0090] This embodiment provides a method for extracting iron and aluminum from wet-process phosphoric acid in steps. The method is the same as that of Embodiment 1 except that the second extraction is a single-stage extraction.

[0091] 2. Comparison

[0092] Comparative Example 1

[0093] This comparative example provides a method for extracting iron and aluminum from wet-process phosphoric acid. The method is the same as Example 1 except that the volume ratio of the first extraction system to the wet-process phosphoric acid is 5:1.

[0094] Comparative Example 2

[0095] This comparative example provides a method for extracting iron and aluminum from wet-process phosphoric acid, which is the same as Example 1 except that the volume ratio of the second extraction system to the iron-removing phosphoric acid is 1:1.

[0096] 3. Test and its results

[0097] The extraction rates of iron ions and aluminum ions in the methods provided in the above embodiments and comparative examples were tested and calculated respectively, and the results are shown in Table 2;

[0098] Table 2

[0099]

[0100]

[0101] From Table 2 we can see that:

[0102] (1) It can be seen from Examples 1 to 3 that the present invention adjusts the O / A ratio of the first extraction and the second extraction, extracts the iron ions in the wet-process phosphoric acid at a lower O / A ratio, and further extracts the aluminum ions in the iron-free phosphoric acid at a higher O / A ratio, thereby achieving step-by-step extraction of iron ions and aluminum ions in the wet-process phosphoric acid, and the extraction rate of iron ions is as high as 95.31% or more, and the extraction rate of aluminum ions is as high as 85.90% or more; so that aluminum ions and iron ions with similar properties can be recovered separately in the subsequent process, which is conducive to the high-quality utilization of the subsequent iron-free aluminum phosphoric acid.

[0103] (2) It can be seen from Examples 1 and 4 to 7 that, due to the high volume ratio of the first extraction system to wet-process phosphoric acid in Example 4, the iron ions and aluminum ions in the wet-process phosphoric acid are extracted simultaneously in the first extraction process of step (1), and cannot be recovered separately; while in Example 5, the volume ratio of the first extraction system to wet-process phosphoric acid is low, resulting in the iron ion extraction rate being reduced to 65.02%, and iron ions still remaining in the iron-free phosphoric acid; due to the low volume ratio of the second extraction system to the iron-free phosphoric acid in Example 6, the aluminum ion extraction is incomplete, and the aluminum ion extraction rate is reduced to 70.51%; while in Example 7, the volume ratio of the second extraction system to the iron-free phosphoric acid is high, and the aluminum ion extraction effect is not significantly improved, but the extractant is wasted; thus, the present invention further preferably has a volume ratio of the first extraction system to the wet-process phosphoric acid of 1:(1-3), and preferably has a volume ratio of the second extraction system to the iron-free phosphoric acid of (4-6):1, and the synergistic combination further improves the efficient extraction and selective separation and recovery of iron ions and aluminum ions in the wet-process phosphoric acid.

[0104] (3) It can be seen from Example 1 and Example 8 that since the diluent content in the first extraction system in Example 8 is relatively large, the iron ion extraction effect is poor, only 81.24%, and some iron ions still remain; the present invention further preferably has a volume ratio of the extractant to the diluent in the first extraction system of 1: (0.5-1.5), which further improves the extraction effect of iron ions and aluminum ions in wet-process phosphoric acid.

[0105] (4) It can be seen from Examples 1 and 9 to 10 that the second stirring rate in the second extraction process in Example 9 is relatively low, and the extraction rate of aluminum ions decreases to 84.22%; the second extraction in Example 10 is a single-stage extraction, resulting in a poor extraction effect of aluminum ions, which decreases to 46.19%; it can be seen that the present invention further optimizes the extraction temperature, stirring rate and extraction stage in the second extraction process, and further improves the extraction rate of aluminum ions in wet-process phosphoric acid.

[0106] (5) It can be seen from Example 1 and Comparative Examples 1 to 2 that, since the first extraction and the second extraction in Comparative Example 1 are both carried out under a relatively large O / A ratio, both iron ions and aluminum ions are extracted in the first extraction process, making it difficult to achieve separate extraction and recovery of iron ions and aluminum ions in wet-process phosphoric acid; and in Comparative Example 2, both the first extraction and the second extraction are carried out under a relatively small O / A ratio, resulting in insufficient extraction of aluminum ions or almost no extraction of aluminum ions in the second extraction process, making it impossible to achieve recovery and reuse of aluminum ions in wet-process phosphoric acid.

[0107] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for extracting iron and aluminum from wet-process phosphoric acid in steps, characterized in that: The method comprises the following steps: (1) mixing the first extraction system and wet-process phosphoric acid in a volume ratio of 1:(1-6) to perform a first extraction to obtain iron-removing phosphoric acid; (2) mixing the second extraction system and the iron-removing phosphoric acid described in step (1) at a volume ratio of (1.2-6):1 to perform a second extraction to obtain the iron-removing aluminum phosphoric acid; Wherein, the first extraction system and the second extraction system each independently comprise an extractant containing phosphorus-oxygen double bonds and / or an extractant containing phosphorus-hydroxyl groups.

2. The method according to claim 1, characterized in that Step (1) The volume ratio of the first extraction system to the wet-process phosphoric acid is 1:(1-3); Preferably, the volume ratio of the second extraction system in step (2) to the iron-removing phosphoric acid in step (1) is (4-6):

1.

3. The method according to claim 1 or 2, characterized in that: In terms of mass percentage, the content of iron ions in the wet-process phosphoric acid in step (1) is 0.10-0.50 wt %; Preferably, the content of aluminum ions in the wet-process phosphoric acid in step (1) is 0.60 to 3.0 wt % in terms of mass percentage.

4. The method according to any one of claims 1 to 3, characterized in that: The extractant containing phosphorus-oxygen double bonds includes any one of trialkylphosphine oxide, tributyl phosphate, Cyanex 272, dimethylheptyl methylphosphonate or 2-ethylhexyl diphenyl phosphate, or a combination of at least two thereof; Preferably, the extractant containing phosphorus hydroxyl groups comprises di(2-ethylhexyl) phosphate and / or 2-ethylhexyl phosphate.

5. The method according to any one of claims 1 to 4, characterized in that: Step (1) The first extraction system also includes a first diluent; Preferably, the volume ratio of the extractant to the first diluent in the first extraction system is 1:(1-4), preferably 1:(1-2); Preferably, the second extraction system in step (2) further includes a second diluent; Preferably, the volume ratio of the extractant to the second diluent in the second extraction system is 1:(1-4); Preferably, the first diluent and the second diluent each independently include any one of kerosene, sulphonated kerosene, cyclohexane, xylene, n-heptane or ethyl acetate, or a combination of at least two thereof.

6. The method according to any one of claims 1 to 5, characterized in that: Step (1) The temperature of the first extraction is 20-50° C.; Preferably, the first extraction time in step (1) is 5 to 30 minutes; Preferably, the first extraction in step (1) is accompanied by a first stirring; Preferably, the first stirring rate is 50-200 r / min, preferably 100-180 r / min.

7. The method according to any one of claims 1 to 6, characterized in that: Step (2) The temperature of the second extraction is 20 to 90° C., preferably 60 to 90° C.; Preferably, the second extraction time in step (2) is 5 to 60 minutes; Preferably, the second extraction process in step (2) is accompanied by a second stirring; Preferably, the second stirring rate is 50-300 r / min, preferably 200-300 r / min.

8. The method according to any one of claims 1 to 7, characterized in that: The first extraction and the second extraction methods independently include single-stage extraction and / or multi-stage extraction; preferably, the first extraction method is single-stage extraction; preferably, the second extraction method is multi-stage extraction; Preferably, the extraction stages of the multi-stage extraction are 2 to 5.

9. The method according to any one of claims 1 to 8, characterized in that: Step (1) after the first extraction, an iron-loaded extractant is obtained; Preferably, after the second extraction in step (2), an extractant loaded with aluminum is obtained.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) mixing the first extraction system and wet-process phosphoric acid at a volume ratio of 1:(1-6), performing a first extraction for 5-30 minutes at 20-50° C. and a first stirring rate of 50-200 r / min to obtain iron-removing phosphoric acid and an iron-loaded extractant; (2) mixing the second extraction system with the iron-removing phosphoric acid described in step (1) at a volume ratio of (1.2-6):1, performing a second extraction for 5-60 minutes at 20-90° C. and a second stirring rate of 50-300 r / min to obtain an iron-removing aluminum phosphoric acid and an aluminum-loaded extractant; Wherein, the content of iron ions in the wet-process phosphoric acid in step (1) is 0.10-0.50wt%, and the content of aluminum ions is 0.60-3.0wt%; the first extraction and the second extraction methods each independently include single-stage extraction and / or multi-stage extraction, and the number of stages of the multi-stage extraction is 2-5; The first extraction system and the second extraction system each independently include an extractant containing a phosphorus-oxygen double bond and / or an extractant containing a phosphorus hydroxyl group; the first extraction system also includes a first diluent; the volume ratio of the extractant to the first diluent in the first extraction system is 1:(1-4); the second extraction system also includes a second diluent; the volume ratio of the extractant to the second diluent in the second extraction system is 1:(1-4).

Citation Information

Patent Citations

  • Method for reducing iron and aluminum ions in wet phosphoric acid

    CN101920946B

  • Method for removing iron through wet-method phosphoric acid purification

    CN110116997A

  • Method for extracting and grouping-separating light, middle and heavy rare earth elements in multi-rare earth complex solution

    CN103122410A

  • Method for extracting and separating iron and aluminum from hydrochloric acid media

    CN104946889A

  • Extracting agent for extracting iron and aluminum in wet-process phosphoric acid liquor as well as preparation method and application of extracting agent