Process for smelting metallic silicon by petroleum coke

By pretreatment and process parameters of silica and petroleum coke, combined with the use of calcium fluoride, magnesium oxide and argon chlorine, the problems of low smelting efficiency and environmental pollution in petroleum coke smelting metal silicon process are solved, and high purity is achieved. High efficiency of metal silicon production and environmental protection.

CN119059524APending Publication Date: 2024-12-03XINJIANG WEST HESHENG SILICON MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411338792.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing petroleum coke smelting metal silicon process has problems such as low smelting efficiency, unstable product quality, high energy consumption and a great impact on the environment.

Method used

By pretreating silica and petroleum coke, optimizing the batching ratio, using calcium fluoride and magnesium oxide as flux and antioxidants, controlling the smelting conditions of the electric furnace, refining with argon and chlorine, combining casting and exhaust gas treatment technologies, ensuring the process Real-time monitoring and automatic optimization of parameters.

Benefits of technology

It improves the purity and output of metal silicon, reduces raw material and energy consumption costs, reduces environmental pollution, and ensures the stability of the smelting process and the consistency of product quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of metallic silicon smelting, and discloses a process for smelting metallic silicon from petroleum coke, which comprises the following steps: pretreating a silica raw material, crushing the silica raw material into particles with the particle size of 20-80mm, and carrying out magnetic separation to remove iron so as to reduce the iron content in silica and improve the purity of metallic silicon; meanwhile, the petroleum coke is ground, so that the particle size of the petroleum coke reaches 30-100 meshes, the specific surface area of the petroleum coke is increased, and the reaction activity of the petroleum coke is improved. According to the method, silica and petroleum coke can be fully reacted, impurities can be effectively removed, the purity and yield of metal silicon can be improved by pretreating silica and petroleum coke, optimizing the proportioning proportion and accurately controlling technological parameters in the smelting and refining process, the petroleum coke is adopted as a reducing agent, and compared with a traditional reducing agent, the petroleum coke is relatively low in price, and the cost is low. The source is wide, and the raw material cost can be reduced. In addition, by optimizing process parameters, the smelting efficiency is improved, and the energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallic silicon smelting, and in particular to a process for smelting metallic silicon from petroleum coke. Background Art

[0002] Metallic silicon, also known as crystalline silicon or industrial silicon, is mainly used as an additive for non-ferrous alloys. Metallic silicon is a product smelted from quartz and coke in an electric furnace. The content of the main component silicon is about 98% (in recent years, silicon with a content of 99.99% is also included in metallic silicon), and the remaining impurities are iron, aluminum, calcium, etc.

[0003] With the development of the petroleum industry, petroleum coke, as a by-product of petroleum refining, has high carbon content, relatively low price and wide sources. The application of petroleum coke in metal silicon smelting is expected to solve the problems caused by traditional reducing agents, but the current petroleum coke metal silicon smelting process still has some shortcomings, such as poor smelting efficiency, unstable product quality, high energy consumption and certain impact on the environment. Therefore, it is necessary to improve and perfect the petroleum coke metal silicon smelting process. For this purpose, a petroleum coke metal silicon smelting process that solves the above problems is proposed. Summary of the invention

[0004] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions: A process for smelting metallic silicon from petroleum coke comprises the following steps: pre-treating silica raw material, crushing it into particles with a particle size of 20-80 mm, and performing magnetic separation to remove iron, so as to reduce the iron content in the silica and improve the purity of metallic silicon; at the same time, grinding the petroleum coke to make its particle size reach 30-100 meshes, so as to increase the specific surface area of ​​the petroleum coke and improve its reaction activity.

[0005] Furthermore, during the batching process, the pretreated silica and petroleum coke are mixed in a mass ratio of 10:3 - 10:4, and 2% - 5% of the total mass of the mixture is added as a flux to reduce the reaction temperature and improve the smelting efficiency; in addition, 0.5% - 1% of the total mass of the mixture is added as an antioxidant to reduce the oxidation loss of metallic silicon during the smelting process.

[0006] Furthermore, it is required that during the electric furnace smelting process, the mixed material is uniformly added into the electric furnace, the heating power of the electric furnace is controlled so that the temperature in the furnace is between 1900-2100°C, the current intensity is between 8000-12000A, and the voltage is between 120-180V; at the same time, a continuous feeding and discharging method is adopted to maintain the dynamic balance of the materials in the furnace, and the smelting time is 10-15 hours, so that the silica and petroleum coke can fully react to generate metallic silicon liquid and slag.

[0007] Furthermore, during the refining process, the smelted metallic silicon liquid is transferred to a refining furnace, and a mixed gas of argon and chlorine is introduced into the furnace for stirring and refining, wherein the volume ratio of argon to chlorine is 5:1 - 10:1, and the ventilation time is 1 - 2 hours; the impurity elements in the metallic silicon liquid, such as aluminum, calcium, titanium, etc., are removed by the strong oxidizing property of chlorine, thereby improving the purity of the metallic silicon; at the same time, the introduction of argon can play a stirring role, making the reaction more uniform.

[0008] Furthermore, the insulation temperature during the refining process is controlled between 1600-1700°C and the insulation time is 2-3 hours; during the insulation process, impurities in the metal silicon liquid further float and condense to form scum; by regularly removing the scum, impurities in the metal silicon liquid can be effectively removed and the quality of the metal silicon can be improved; after the insulation is completed, the metal silicon liquid is allowed to stand for a period of time to allow the tiny impurity particles therein to fully precipitate, thereby further improving the purity of the metal silicon.

[0009] Furthermore, in the casting step, a high-temperature resistant graphite mold is used as a casting container, and the refined metallic silicon liquid is slowly cast into the mold at a temperature of 1450-1550°C; during the casting process, the casting speed and flow rate are controlled to avoid splashing and bubbles in the metallic silicon liquid to ensure the casting quality; after the casting is completed, the metallic silicon ingot is allowed to cool naturally in the mold to room temperature, and then demolded and taken out.

[0010] Furthermore, in the crushing and screening process, the cooled metal silicon ingots are crushed in two stages by a jaw crusher and a cone crusher to crush them into small pieces with a particle size of 50-100mm; then, the crushed materials are screened by a vibrating screen, and the materials that do not meet the particle size requirements are returned to the crusher for re-crushing until a metal silicon product with a particle size of 10-100mm is obtained; in the crushing and screening process, attention should be paid to controlling the generation of dust, and measures such as water spraying and dust suction devices should be adopted to reduce environmental pollution.

[0011] Furthermore, the waste gas generated in the process mainly includes smoke generated during electric furnace smelting and chlorine-containing gas generated during refining. For the treatment of waste gas, a bag filter and a wet scrubber are used to purify the waste gas. First, the smoke particles in the waste gas are removed by a bag filter. Then the waste gas is passed into a wet scrubber and the chlorine-containing gas therein is absorbed by a sodium hydroxide solution. The waste gas is discharged after meeting the national emission standards.

[0012] Furthermore, during the entire smelting process, various process parameters are monitored in real time and data is collected through detection equipment such as temperature sensors, pressure sensors, current sensors and voltage sensors installed on electric furnaces, refining furnaces and casting equipment; the collected data is transmitted to the central control system, and the data is analyzed and processed by computer software. According to the analysis results, the operating parameters of the smelting equipment are automatically adjusted and optimized to ensure the stability of the smelting process and the consistency of product quality.

[0013] Furthermore, the metal silicon products after smelting are subjected to quality inspection, and the inspection items include chemical composition analysis, physical property inspection and appearance quality inspection, etc.; the chemical composition analysis mainly detects the silicon content and impurity element content in the metal silicon; the physical property inspection mainly detects the hardness, density, melting point, etc. of the metal silicon; the appearance quality inspection mainly checks whether the surface of the metal silicon is smooth, and whether there are cracks and inclusions, etc.; through strict quality inspection, it is ensured that the products meet national standards and customer requirements, and the market competitiveness of the products is improved. Beneficial Effects

[0014] 1. This petroleum coke smelting metal silicon process can make silica and petroleum coke fully react, effectively remove impurities, and improve the purity and yield of metal silicon by pre-treating silica and petroleum coke, optimizing the proportion of ingredients, and accurately controlling the process parameters during smelting and refining. Petroleum coke is used as a reducing agent. Compared with traditional reducing agents, petroleum coke is relatively cheap and widely available, which can reduce the cost of raw materials. In addition, by optimizing process parameters, improving smelting efficiency, and reducing energy consumption, production costs can also be further reduced.

[0015] 2. This petroleum coke smelting metal silicon process can effectively reduce environmental pollution by purifying the smoke and chlorine-containing gas generated during the smelting process through the waste gas treatment system, so that it can be discharged after meeting the national emission standards. At the same time, by optimizing the process and reducing the generation of waste slag, it is also beneficial to environmental protection. Through various sensors installed on the smelting equipment, the process parameters are monitored and data collected in real time, and the data is analyzed and processed through the central control system to achieve automatic adjustment and optimization of the operating parameters of the smelting equipment, which can ensure the stability of the smelting process and the consistency of product quality. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0017] A process for smelting metallic silicon from petroleum coke, characterized in that it includes the following steps: pretreating the silica raw material, crushing it into particles with a particle size of 20-80 mm, and performing magnetic separation to remove iron to reduce the iron content in the silica and improve the purity of the metallic silicon; at the same time, grinding the petroleum coke to a particle size of 30-100 meshes to increase the specific surface area of ​​the petroleum coke and improve its reaction activity. The process for smelting metallic silicon from petroleum coke according to claim 1 is characterized in that in the batching process, the pretreated silica and petroleum coke are mixed in a mass ratio of 10:3-10:4, and calcium fluoride accounting for 2%-5% of the total mass of the mixture is added as a flux to reduce the reaction temperature and improve the smelting efficiency; in addition, 0.5%-0.5% of the total mass of the mixture is also required to be added. 1% magnesium oxide is used as an antioxidant to reduce the oxidation loss of metallic silicon during the smelting process. A process for smelting metallic silicon from petroleum coke requires that during the smelting process in an electric furnace, the mixed material is evenly added to the electric furnace, the heating power of the electric furnace is controlled, the temperature in the furnace is between 1900-2100°C, the current intensity is between 8000-12000A, and the voltage is between 120-180V; at the same time, a continuous feeding and discharging method is adopted to maintain the dynamic balance of the materials in the furnace, and the smelting time is 10-15 hours, so that silica and petroleum coke can fully react to generate metallic silicon liquid and slag. The process for smelting metallic silicon from petroleum coke according to claim 3 is characterized in that during the refining process, the metallic silicon liquid obtained by smelting is transferred to a refining furnace, and a mixed gas of argon and chlorine is introduced into the furnace for stirring and refining, wherein the volume ratio of argon and chlorine is 5:1-10:1, and the ventilation time is 1- 2 hours; through the strong oxidizing property of chlorine, impurity elements in the metallic silicon liquid, such as aluminum, calcium, titanium, etc., are removed to improve the purity of the metallic silicon; at the same time, the introduction of argon can play a stirring role to make the reaction more uniform, a process for smelting metallic silicon from petroleum coke, wherein the insulation temperature in the refining process is controlled between 1600-1700°C, and the insulation time is 2-3 hours; during the insulation process, the impurities in the metallic silicon liquid further float and condense to form scum; by regularly removing the scum, the impurities in the metallic silicon liquid can be effectively removed to improve the quality of the metallic silicon; after the insulation is completed, the metallic silicon liquid is allowed to stand for a period of time to allow the tiny impurity particles therein to fully precipitate, thereby further improving the purity of the metallic silicon, the process for smelting metallic silicon from petroleum coke according to claim 5, characterized in that in the casting step, a high-temperature resistant graphite mold is used as a casting container, and the refined metallic silicon liquid is cast at 1450- Slowly pour it into the mold at a temperature of 1550℃; during the casting process, control the casting speed and flow rate to avoid splashing and bubbles in the metal silicon liquid to ensure the casting quality;After the casting is completed, the metal silicon ingot is allowed to cool naturally in the mold to room temperature, and then demolded and taken out. A process for smelting metal silicon from petroleum coke. In the crushing and screening stages, a jaw crusher and a cone crusher are used to crush the cooled metal silicon ingot in two stages to crush it into small pieces with a particle size of 50-100mm; then, the crushed material is screened by a vibrating screen, and the material that does not meet the particle size requirements is returned to the crusher for re-crushing until a particle size of 10- 100mm metallic silicon products; in the process of crushing and screening, attention should be paid to controlling the generation of dust, and measures such as water spraying and dust suction devices should be adopted to reduce environmental pollution. The process for smelting metallic silicon from petroleum coke according to claim 7 is characterized in that the waste gas generated in the process mainly includes smoke generated in the electric furnace smelting process and chlorine-containing gas generated in the refining process; for the treatment of waste gas, a bag filter and a wet scrubber are used to purify the waste gas; first, the smoke particles in the waste gas are removed by a bag filter, and then the waste gas is passed into a wet scrubber, and the chlorine-containing gas therein is absorbed by a sodium hydroxide solution, so that the waste gas meets the national emission standards before being discharged. A process for smelting metallic silicon from petroleum coke, in which, during the entire smelting process, temperature sensors, pressure sensors installed in the electric furnace, refining furnace and casting equipment are used to detect the presence of dust in the waste gas. Sensors, current sensors, voltage sensors and other detection equipment are used to monitor and collect data of various process parameters in real time; the collected data is transmitted to the central control system, the data is analyzed and processed by computer software, and the operating parameters of the smelting equipment are automatically adjusted and optimized according to the analysis results to ensure the stability of the smelting process and the consistency of product quality. According to claim 9, the process of smelting metal silicon from petroleum coke is characterized in that the metal silicon product after smelting is subjected to quality inspection, and the inspection items include chemical composition analysis, physical property inspection and appearance quality inspection, etc.; chemical composition analysis mainly detects the silicon content and impurity element content in metal silicon; physical property inspection mainly detects the hardness, density, melting point, etc. of metal silicon; appearance quality inspection mainly checks whether the surface of metal silicon is smooth, whether there are cracks and inclusions, etc.;

[0018] Working principle: 1. Raw material pretreatment Silica pretreatment The silica ore is crushed and crushed into particles with a size of 20 - 80 mm using a jaw crusher.

[0019] The crushed silica particles are subjected to magnetic separation to remove iron. A magnetic separator is used to remove iron impurities, reduce the iron content in the silica, and improve the purity of subsequent metallic silicon.

[0020] Petroleum coke processing The petroleum coke is put into a ball mill for grinding to a particle size of 30-100 mesh. By increasing the specific surface area of ​​the petroleum coke, its reactivity in the smelting process is improved.

[0021] 2. Ingredients The pretreated silica and petroleum coke are placed in a mixer at a mass ratio of 10:3 - 10:4 for mixing.

[0022] During the mixing process, calcium fluoride accounting for 2% - 5% of the total mass of the mixture is added as a flux to reduce the reaction temperature and improve the smelting efficiency.

[0023] At the same time, 0.5% - 1% of magnesium oxide is added to the total mass of the mixture as an antioxidant to reduce the oxidation loss of metallic silicon during the smelting process.

[0024] 3. Electric furnace smelting The uniformly mixed materials are continuously added into the electric furnace through the feeding device.

[0025] Control the heating power of the electric furnace so that the temperature inside the furnace gradually increases to 1900 - 2100℃, the current intensity is maintained at 8000 - 12000A, and the voltage is controlled at 120 - 180V.

[0026] The continuous feeding and discharging method is adopted to maintain the dynamic balance of the materials in the furnace. During the smelting process, silica and petroleum coke react fully to produce metallic silicon liquid and slag. The smelting time is 10-15 hours.

[0027] 4. Refining The metallic silicon liquid obtained by smelting in the electric furnace is transferred to the refining furnace.

[0028] A mixed gas of argon and chlorine is introduced into the refining furnace, wherein the volume ratio of argon to chlorine is 5:1 - 10:1. The ventilation time is 1 - 2 hours. The strong oxidizing property of chlorine removes impurity elements in the metal silicon liquid, such as aluminum, calcium, titanium, etc. At the same time, the introduction of argon plays a stirring role, making the reaction more uniform.

[0029] The holding temperature during the refining process is controlled at 1600-1700℃ for 2-3 hours. During the holding process, the impurities in the metal silicon liquid further float and condense to form scum. The scum is removed regularly to remove the impurities in the metal silicon liquid. After the holding is completed, the metal silicon liquid is left to stand for a period of time to allow the tiny impurity particles in it to fully settle.

[0030] 5. Casting Use high temperature resistant graphite mold as casting container.

[0031] The refined metal silicon liquid is slowly cast into the graphite mold through the casting equipment at a temperature of 1450-1550℃. During the casting process, the casting speed and flow rate should be controlled to avoid splashing and bubbles in the metal silicon liquid to ensure the casting quality.

[0032] After the casting is completed, the metal silicon ingot is allowed to cool naturally to room temperature in the mold, and then demolding operation is performed to take out the metal silicon ingot.

[0033] 6. Crushing and Screening The cooled metal silicon ingot is crushed in two stages using a jaw crusher and a cone crusher to crush it into small pieces with a particle size of 50-100mm.

[0034] The crushed materials are screened by a vibrating screen, and the materials that do not meet the particle size requirements are returned to the crusher for re-crushing until metallic silicon products with a particle size of 10-100mm are obtained.

[0035] During the crushing and screening process, measures such as water spraying and dust suction devices are used to control dust generation and reduce environmental pollution.

[0036] 7. Waste gas treatment The smoke and dust generated during the electric furnace smelting process is collected through the pipeline and enters the bag filter for treatment. The filter bags in the bag filter intercept the smoke and dust particles, and the purified gas is discharged into the atmosphere.

[0037] The chlorine-containing gas generated during the refining process is introduced into the wet scrubber through a pipeline. In the scrubber, sodium hydroxide solution is used as an absorbent to react with the chlorine-containing gas, converting the chlorine element in it into substances such as sodium chloride, thereby achieving the purpose of purifying the waste gas. The purified waste gas is discharged after meeting the national emission standards.

[0038] 8. Process parameter monitoring and control Temperature sensors, pressure sensors, current sensors, voltage sensors and other detection equipment are installed on electric furnaces, refining furnaces and casting equipment to monitor various process parameters in real time.

[0039] The detection equipment transmits the collected data to the central control system, and the computer software in the central control system analyzes and processes the data.

[0040] Based on the analysis results, the central control system automatically adjusts and optimizes the operating parameters of the smelting equipment to ensure the stability of the smelting process and the consistency of product quality.

[0041] IX. Quality Inspection The chemical composition of the metal silicon product after smelting is analyzed, and the silicon content and the content of impurity elements (such as iron, aluminum, calcium, titanium, etc.) in the metal silicon are detected by a spectrometer.

[0042] Physical property tests are carried out, the hardness of metal silicon is measured using a hardness tester, its density is measured using a densitometer, its melting point is detected using a melting point tester, and appearance quality inspection is carried out to observe whether the surface of the metal silicon is smooth and whether there are defects such as cracks and inclusions.

[0043] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for smelting metallic silicon from petroleum coke, characterized in that: The following steps are involved: The silica raw material is pretreated and crushed into particles with a size of 20-80mm, and magnetic separation is performed to remove iron to reduce the iron content in the silica and improve the purity of metallic silicon; at the same time, the petroleum coke is ground to a particle size of 30-100 mesh to increase the specific surface area of ​​the petroleum coke and improve its reaction activity.

2. The process for smelting metallic silicon from petroleum coke according to claim 1, characterized in that: During the batching process, the pretreated silica and petroleum coke are mixed in a mass ratio of 10:3 - 10:4, and calcium fluoride accounting for 2% - 5% of the total mass of the mixture is added as a flux to reduce the reaction temperature and improve the smelting efficiency; in addition, magnesium oxide accounting for 0.5% - 1% of the total mass of the mixture is added as an antioxidant to reduce the oxidation loss of metallic silicon during the smelting process.

3. The process for smelting metallic silicon from petroleum coke according to claim 2, characterized in that The mixed material is added evenly into the electric furnace, and the heating power of the electric furnace is controlled to make the temperature in the furnace between 1900-2100℃, the current intensity between 8000-12000A, and the voltage between 120-180V; at the same time, the dynamic balance of the materials in the furnace is maintained by continuous feeding and discharging. The smelting time is 10-15 hours to allow the silica and petroleum coke to fully react to generate metallic silicon liquid and slag.

4. The process for smelting metallic silicon from petroleum coke according to claim 3, characterized in that: During the refining process, the smelted metallic silicon liquid is transferred to a refining furnace, and a mixed gas of argon and chlorine is introduced into the furnace for stirring and refining, wherein the volume ratio of argon to chlorine is 5:1 - 10:1, and the ventilation time is 1 - 2 hours; the strong oxidizing property of chlorine is used to remove impurity elements in the metallic silicon liquid, such as aluminum, calcium, titanium, etc., to improve the purity of the metallic silicon; at the same time, the introduction of argon can play a stirring role to make the reaction more uniform.

5. The process for smelting metallic silicon from petroleum coke according to claim 4, characterized in that: The insulation temperature during the refining process is controlled between 1600-1700℃ and the insulation time is 2-3 hours. During the insulation process, impurities in the metal silicon liquid further float and condense to form scum. By regularly removing the scum, impurities in the metal silicon liquid can be effectively removed and the quality of the metal silicon can be improved. After the insulation is completed, the metal silicon liquid is left to stand for a period of time to allow the tiny impurity particles in it to fully precipitate, further improving the purity of the metal silicon.

6. The process for smelting metallic silicon from petroleum coke according to claim 5, characterized in that: In the casting step, a high-temperature resistant graphite mold is used as a casting container, and the refined metallic silicon liquid is slowly cast into the mold at a temperature of 1450-1550°C; during the casting process, the casting speed and flow rate must be controlled to avoid splashing and bubbles in the metallic silicon liquid to ensure the casting quality; after the casting is completed, the metallic silicon ingot is allowed to cool naturally in the mold to room temperature, and then demolded and taken out.

7. The process for smelting metallic silicon from petroleum coke according to claim 6, characterized in that: The cooled metal silicon ingots are crushed in two stages using a jaw crusher and a cone crusher to crush them into small pieces with a particle size of 50-100mm. Then, the crushed materials are screened using a vibrating screen, and the materials that do not meet the particle size requirements are returned to the crusher for re-crushing until metal silicon products with a particle size of 10-100mm are obtained. During the crushing and screening process, attention should be paid to controlling the generation of dust, and measures such as water spraying and dust suction devices should be adopted to reduce environmental pollution.

8. The process for smelting metallic silicon from petroleum coke according to claim 7, characterized in that: The waste gas generated in this process mainly includes smoke generated during electric furnace smelting and chlorine-containing gas generated during refining. For the treatment of waste gas, a bag filter and a wet scrubber are used to purify it. First, the smoke particles in the waste gas are removed by a bag filter, and then the waste gas is passed into a wet scrubber to absorb the chlorine-containing gas therein with sodium hydroxide solution, so that the waste gas meets the national emission standards before being discharged.

9. The process for smelting metallic silicon from petroleum coke according to claim 8, characterized in that: During the entire smelting process, various process parameters are monitored in real time and data is collected through detection equipment such as temperature sensors, pressure sensors, current sensors and voltage sensors installed on electric furnaces, refining furnaces and casting equipment. The collected data is transmitted to the central control system, analyzed and processed by computer software, and the operating parameters of the smelting equipment are automatically adjusted and optimized based on the analysis results to ensure the stability of the smelting process and the consistency of product quality.

10. The process for smelting metallic silicon from petroleum coke according to claim 9, characterized in that: The metal silicon products after smelting are subjected to quality inspection, and the inspection items include chemical composition analysis, physical property inspection and appearance quality inspection, etc.; the chemical composition analysis mainly detects the silicon content and impurity element content in the metal silicon; the physical property inspection mainly detects the hardness, density, melting point, etc. of the metal silicon; the appearance quality inspection mainly checks whether the surface of the metal silicon is smooth, and whether there are cracks and inclusions, etc.

Citation Information

Patent Citations

  • Silica reduction method for producing silicon

    CN101555011A

  • Method for removing impurity phosphorus in silicon

    CN102020278A

  • Method for reextracting metallic silicon from metallic silicon residues

    CN104909367A

  • Metal silicon smelting method

    CN108862280A

  • Production process for smelting metallic silicon by using full oil coke

    CN111410198A