Metal-containing ZSM-5 molecular sieve as well as preparation method and application thereof
By mixing the active metal source with peroxide in a silicon-aluminum-type ZSM-5 molecular sieve with uniform distribution of active metals, the metal-containing ZSM-5 molecular sieve was prepared, which solved the problems of metal packaging difficulties and reduced activity, and improved the problem of improved metallic packaging The low-carbon olefin yield and catalytic properties of diesel catalytic cracking reaction are obtained.
Patent Information
- Application Number
- CN202310640038.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
In the prior art, there are few studies on encapsulation of metals into silicon-aluminum-type MFI molecular sieves, especially in high-temperature reactions, metal particles are prone to particle aggregation or inactivation, and nickel, as a dehydrogenation component, is also a catalytic calcification poison, and is used to limit.
By using a method without using amine nitrogen organics and amine nitrogen ligands, the active metal source and peroxide and silicon-aluminum ZSM-5 molecular sieve are mixed through hydrothermal reaction to prepare metal-containing ZSM-5 with uniform distribution of active metals. Molecular sieve, used for catalytic cracking reaction of diesel.
It realizes the preparation of clean and pollution-free molecular sieve, and the distribution of active metals is uniformly, which improves the yield of low-carbon olefins, and reduces the harshness of diesel catalytic cracking reaction, improving catalytic performance.
Smart Images

Figure CN119059530A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a metal-containing ZSM-5 molecular sieve and a preparation method and application thereof. Background Art
[0002] Catalytic cracking refers to the process of converting hydrocarbons into low-carbon olefins such as ethylene, propylene and butene under the action of a catalyst, and producing light aromatics at the same time. The process of producing low-carbon olefins by catalytic cracking of heavy oil has always occupied a large share of the low-carbon olefin market due to its strong raw material adaptability and low production cost. Since the mid-1980s, Sinopec Research Institute of Petroleum and Chemical Industry (Sinopec Research Institute) has been tracking and studying this technology. In 1994, the Research Institute of Petroleum and Chemical Industry developed a catalytic cracking (DCC) process for producing low-carbon olefins using heavy oil (vacuum distillate oil, coking gas oil and residual oil, etc.) as raw materials. After the successful industrialization of DCC technology, the Research Institute of Petroleum and Chemical Industry developed a catalytic thermal cracking (CPP) process for directly producing ethylene and propylene from heavy oil, which has multiple production schemes such as maximum ethylene, maximum propylene and simultaneous production of ethylene and propylene. Compared with the steam cracking process, the CPP process broadens the source of ethylene raw materials and reduces the cost of ethylene raw materials. At the same time, the reaction temperature is lower than that of the steam cracking process, so the energy consumption of the device is significantly reduced. Light oil catalytic cracking mainly refers to the process of producing ethylene and propylene from light gasoline or naphtha in the presence of a catalyst. This process can realize the transformation of petroleum resources into basic chemical raw materials and will play an important role in future chemical refineries.
[0003] ZSM-5 molecular sieve is a silicon-aluminum type MFI molecular sieve with a specific three-dimensional ten-membered ring pore structure and suitable acid properties. It shows good propylene selectivity. At the same time, it has good hydrothermal stability and inhibition of coke precursors. It is one of the most promising active components of catalytic cracking catalysts. The acid properties of molecular sieves include factors such as acid type, acid amount, acid strength and acid center distribution. Element modification is a simple and effective method to adjust the acidity of molecular sieves. Studies have modified ZSM-5 molecular sieves with alkaline earth metals such as Mg, Ca, Ba and Sr. It was found that the introduction of alkaline earth metals promoted the transformation of some strong acid sites into weak acid sites. When n-butane was used as a reactant, the introduction of Ba obtained the highest ethylene and propylene yields, while the aromatic yield decreased significantly, which may be due to the inhibition of hydrogen transfer reactions. However, in high-temperature reactions, metal particles tend to aggregate or become inactivated due to metal leaching.
[0004] There are methods for encapsulating metals into all-silicon or high-silicon MFI molecular sieves in the prior art, but there are relatively few studies on encapsulating metals into silicon-aluminum MFI molecular sieves. This is because if the metal is directly introduced into the synthesis system, it is easy for the metal to form hydroxide precipitation in an alkaline environment, and the metal easily interacts with phosphorus, resulting in difficult synthesis or low activity. In addition, nickel, as a dehydrogenation component, has a certain dehydrogenation effect, but because it is also a poison for catalytic cracking, its application is greatly limited. Summary of the invention
[0005] The purpose of the present disclosure is to provide a metal-containing ZSM-5 molecular sieve and a preparation method and application thereof. The method does not use amine nitrogen organic matter and amine nitrogen ligands, does not discharge amine nitrogen wastewater, is clean and pollution-free, and the prepared molecular sieve has uniform distribution of active metals. It is used for catalytic cracking reaction of diesel and has a better yield of light olefins.
[0006] In order to achieve the above object, the present disclosure provides a method for preparing a metal-containing ZSM-5 molecular sieve in a first aspect, the method comprising:
[0007] S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture;
[0008] S2, mixing the active metal source, peroxide, water and the first mixture and performing a hydrothermal reaction;
[0009] Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent; the metal in the active metal source is one or more of nickel, copper, zinc, manganese, lanthanum and cerium.
[0010] Optionally, step S2 includes:
[0011] SS1. Mixing the active metal source, peroxide and water to obtain a second mixture; the molar ratio of the active metal source, peroxide and water in terms of metal oxide is 1:(0.2-3.5):(300-1400), preferably 1:(0.3-2.7):(500-1200)
[0012] SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as the metal oxide is 1:(0.1-2.0), preferably 1:(0.3-1.5).
[0013] Optionally, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (30-100):1:(2-15):(300-1500), preferably (35-70):1:(2-10):(350-1000);
[0014] Calculated as SiO2, the amount of the seed crystal used is 1-15 wt%, preferably 8-10 wt%, relative to the total weight of the silicon source.
[0015] Optionally, in step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C., and time of 8-32 h.
[0016] Optionally, the method further comprises: subjecting the solid product obtained by the hydrothermal treatment to ammonium exchange and calcination treatment; the conditions of the calcination treatment comprise: a temperature of 400-800° C., a time of 0.5-8 h, and an atmosphere of air or water vapor.
[0017] Optionally, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate;
[0018] The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate;
[0019] The alkali source includes sodium hydroxide and / or potassium hydroxide;
[0020] The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm;
[0021] The active metal source includes one or more of nickel nitrate, nickel sulfate, nickel hydroxide, copper nitrate, copper sulfate, zinc nitrate, zinc sulfate, manganese nitrate, manganese sulfate, lanthanum nitrate, lanthanum sulfate, cerium nitrate and cerium sulfate.
[0022] A second aspect of the present disclosure provides a metal-containing ZSM-5 molecular sieve prepared by the method provided in the first aspect of the present disclosure.
[0023] Optionally, the metal-containing ZSM-5 molecular sieve has a structure in which an active metal component is encapsulated inside the ZSM-5 molecular sieve; the active metal component is distributed in the pores of the ZSM-5 molecular sieve.
[0024] Optionally, the specific surface area of the metal-containing ZSM-5 molecular sieve is 200-550m 2 / g, with a total pore volume of 0.150-0.22cm 3 ·g -1, the micropore volume is 0.130-0.180cm 3 ·g -1 , the mesopore volume is 0.010-0.100cm 3 ·g -1 , relative crystallinity is 80-100%;
[0025] In the metal-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-100;
[0026] Relative to the total weight of the metal-containing ZSM-5 molecular sieve, the content of the active metal component calculated as metal oxide is 1-3 wt %.
[0027] The third aspect of the present disclosure provides an application of the metal-containing ZSM-5 molecular sieve provided in the second aspect of the present disclosure in a diesel catalytic cracking reaction.
[0028] Optionally, the conditions for the catalytic cracking reaction include: a temperature of 530-720°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1-2.
[0029] Through the above technical scheme, the method disclosed in the present invention does not use amine nitrogen organic matter and amine nitrogen ligands, does not discharge amine nitrogen wastewater, is clean and pollution-free, and the prepared molecular sieve has uniform distribution of active metals. When it is used in the catalytic cracking reaction of diesel, it has a better yield of light olefins.
[0030] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0032] Figure 1 This is the X-ray diffraction spectrum of the copper-containing ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure.
[0033] Figure 2 This is a scanning electron microscope photograph of the copper-containing ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure.
[0034] Figure 3 This is a transmission electron microscope photograph of the copper-containing ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure.
[0035] Figure 4 This is a mapping photo of the copper-containing ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure.
[0036] Figure 5 This is the X-ray diffraction spectrum of the lanthanum-containing ZSM-5 molecular sieve B prepared in Example 2 of the present disclosure.
[0037] Figure 6 This is a scanning electron microscope photograph of the lanthanum-containing ZSM-5 molecular sieve B prepared in Example 2 of the present disclosure.
[0038] Figure 7 This is a mapping photo of the lanthanum-containing ZSM-5 molecular sieve B prepared in Example 2 of the present disclosure.
[0039] Figure 8 This is the X-ray diffraction spectrum of the nickel-containing ZSM-5 molecular sieve F prepared in Example 6 of the present disclosure.
[0040] Fig. 9 This is a scanning electron microscope photograph of the nickel-containing ZSM-5 molecular sieve F prepared in Example 6 of the present disclosure.
[0041] Fig.10 This is a transmission electron microscope photograph of the nickel-containing ZSM-5 molecular sieve F prepared in Example 6 of the present disclosure.
[0042] Fig.11 This is a mapping photo of the nickel-containing ZSM-5 molecular sieve F prepared in Example 6 of the present disclosure.
[0043] Fig.12 This is the X-ray diffraction spectrum of the nickel-containing ZSM-5 molecular sieve G prepared in Example 7 of the present disclosure.
[0044] Fig.13 This is a transmission electron microscope photograph of the nickel-containing ZSM-5 molecular sieve G prepared in Example 7 of the present disclosure.
[0045] Fig.14 This is a mapping photo of the nickel-containing ZSM-5 molecular sieve G prepared in Example 7 of the present disclosure.
[0046] Fig.15 This is the X-ray diffraction spectrum of the nickel-containing ZSM-5 molecular sieve H prepared in Example 8 of the present disclosure. DETAILED DESCRIPTION
[0047] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0048] The first aspect of the present disclosure provides a method for preparing a metal-containing ZSM-5 molecular sieve, the method comprising: S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture; S2, mixing an active metal source, a peroxide, water and the first mixture and then performing a hydrothermal reaction; wherein the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent; and the metal in the active metal source is one or more of nickel, copper, zinc, manganese, lanthanum and cerium.
[0049] The method disclosed in the present invention uses peroxide to synthesize molecular sieves instead of using a template agent containing amine nitrogen, thereby avoiding the discharge of amine nitrogen wastewater, thereby achieving clean production of metal-containing ZSM-5 molecular sieves.
[0050] In a preferred embodiment of the present disclosure, the peroxide is sodium persulfate or hydrogen peroxide, more preferably sodium persulfate. The peroxide can interact with the metal and the molecular sieve precursor at the same time, promote the nucleation of the molecular sieve around the metal, and encapsulate the metal into the interior of the molecular sieve.
[0051] In a specific embodiment of the present disclosure, step S2 includes: SS1, mixing the active metal source, peroxide and water to obtain a second mixture; the molar ratio of the active metal source, peroxide and water in terms of metal oxide is 1: (0.2-3.5): (200-1400), preferably 1: (0.3-2.7): (250-1200), and more preferably 1: (0.35-0.8): (500-1000); SS2, mixing the first mixture with the second mixture and then performing the hydrothermal reaction; the molar ratio of the first mixture in terms of Al2O3 to the second mixture in terms of the metal oxide is 1: (0.1-2.0), preferably 1: (0.15-1.5). Within the above-mentioned dosage ratio range, the second mixture can be free of free metal ions, avoiding the prepared molecular sieve from containing aggregated active metal components, and further improving its catalytic performance.
[0052] In a specific embodiment of the present disclosure, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (30-100):1:(2-15):(300-1500), preferably (35-70):1:(2-10):(350-1000), and more preferably (40-60):1:(4-6):(350-1000); calculated as SiO2, relative to the total weight of the silicon source, the amount of the seed crystal used is 1-15% by weight, preferably 8-10% by weight.
[0053] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art and can be carried out in equipment well known to those skilled in the art, such as a closed heat-resistant and pressure-resistant reactor. In a specific embodiment of the present disclosure, in step S2, the conditions of the hydrothermal reaction include: a temperature of 150-220°C and a time of 8-32h; preferably, a temperature of 150-180°C and a time of 8-20h. The present disclosure does not specifically limit the pressure of the hydrothermal reaction, for example, it can be carried out under the autogenous pressure of the reaction system or under an applied pressure, preferably, under the autogenous pressure of the reaction system.
[0054] In a specific embodiment of the present disclosure, the method further includes: exchanging ammonium and calcining the solid product obtained by the hydrothermal treatment; the conditions of the calcination treatment include: a temperature of 400-800°C, a time of 0.5-8h, and an atmosphere of air atmosphere or water vapor atmosphere; preferably, the temperature is 500-600°C and the time is 2-4h. The calcination treatment is well known to those skilled in the art, and can be carried out in a muffle furnace, a tubular furnace, etc. In a preferred embodiment, the solid product is washed to neutrality before exchanging ammonium, and the liquid used for washing can be any type of liquid that does not react with the solid product, for example, it can be deionized water. In another preferred specific embodiment, the solid obtained by the ammonium exchange is dried before calcination, and the drying conditions can include: a temperature of 100-150°C and a time of 5-20h.
[0055] In a specific embodiment of the present disclosure, the solid product obtained by the hydrothermal treatment can be taken out by centrifugal separation, precipitation and the like.
[0056] According to the present disclosure, the silicon source, aluminum source and alkali source are well known to those skilled in the art. In a specific embodiment of the present disclosure, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; the aluminum source includes one or more of sodium aluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; the alkali source includes sodium hydroxide and / or potassium hydroxide.
[0057] According to the present disclosure, the active metal source can be a water-soluble metal salt, preferably a metal nitrate and / or a metal sulfate of the active metal. In a preferred embodiment, the active metal source includes one or more of nickel nitrate, nickel sulfate, nickel hydroxide, copper nitrate, copper sulfate, zinc nitrate, zinc sulfate, manganese nitrate, manganese sulfate, lanthanum nitrate, lanthanum sulfate, cerium nitrate and cerium sulfate.
[0058] In a specific embodiment of the present disclosure, the seed crystal includes one or more of the ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, for example, including but not limited to ZPR molecular sieve, ZSP molecular sieve, etc.; the average particle size of the ZSM-5 molecular sieve is 0.5-2μm, preferably 1-2μm. The average particle size of the ZSM-5 molecular sieve in the present disclosure refers to the average particle size of the molecular sieve estimated by SEM analysis of the molecular sieve and measuring the particle size of 50 particles randomly selected in the SEM photo to obtain the average value, and the SEM instrument model is HITACHI S-4800.
[0059] A second aspect of the present disclosure provides a metal-containing ZSM-5 molecular sieve prepared by the method provided in the first aspect of the present disclosure.
[0060] In a specific embodiment of the present disclosure, the metal-containing ZSM-5 molecular sieve has a structure in which an active metal component is encapsulated inside the ZSM-5 molecular sieve; the active metal component is distributed in the pores of the ZSM-5 molecular sieve.
[0061] After aging, the metal active components of the molecular sieve disclosed in the present invention are more evenly distributed inside the molecular sieve, which is more conducive to the selective dehydrogenation of alkanes into olefins in the molecular sieve pores, rather than dehydrogenation on the outer surface of the molecular sieve, i.e., confined dehydrogenation. The introduction of metal elements can adjust the acid properties of the ZSM-5 molecular sieve, improve its catalytic function of cracking and dehydrogenation, and introduce the metal active components into the interior of the molecular sieve in an encapsulated manner, further reducing the severity of the diesel catalytic cracking reaction, and improving the conversion rate of saturated hydrocarbons and the selectivity of low-carbon olefins.
[0062] In a specific embodiment of the present disclosure, the specific surface area of the metal-containing ZSM-5 molecular sieve is 200-500m 2 / g, preferably 300-400m 2 / g, with a total pore volume of 0.150-0.22cm 3 ·g -1 , preferably 0.160-0.22cm 3 ·g -1 , the micropore volume is 0.130-0.180cm 3 ·g -1 , preferably 0.140-0.180cm 3 ·g -1 , the mesopore volume is 0.010-0.100cm 3 ·g -1 , preferably 0.010-0.080cm 3 ·g -1 , relative crystallinity is 80-100%, preferably 85-95%;
[0063] In the metal-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-100; relative to the total weight of the metal-containing ZSM-5 molecular sieve, the content of active metal components in terms of metal oxides is 1-3% by weight. Wherein, the molar ratio of SiO2 to Al2O3 can be obtained by X-ray fluorescence spectroscopy. The relative crystallinity is obtained by using a Siemens D5005 X-ray diffractometer based on the standard sample of the ZSM-5 molecular sieve of the Petrochemical Research Institute of China Petrochemical Corporation (i.e., the relative crystallinity of the standard sample of the ZSM-5 molecular sieve of the Petrochemical Research Institute of China Petrochemical Corporation is 100%). The specific surface area and pore volume parameters can be determined by using a specific surface area tester based on the N2 adsorption principle and the BET calculation method (see Petrochemical Analysis Method (RIPP Test Method), RIPP151-90, Science Press, published in 1990). The content of the active iron component in terms of Fe2O3 is obtained by X-ray fluorescence spectroscopy.
[0064] The third aspect of the present disclosure provides an application of the metal-containing ZSM-5 molecular sieve provided in the second aspect of the present disclosure in a diesel catalytic cracking reaction.
[0065] In a specific embodiment of the present disclosure, the conditions of the catalytic cracking reaction include: a temperature of 530-720°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, the agent-oil weight ratio is 1-2; preferably, the temperature is 580-660°C, the reaction mass space velocity is 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1.2-1.9.
[0066] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0067] Silicon-aluminum molar ratio: that is, the molar ratio of SiO2 to Al2O3, tested by X-ray fluorescence spectrometry, the instrument model is Japan Rigaku Electric Co., Ltd. 3013 X-ray fluorescence spectrometer; test conditions: tungsten target, excitation voltage 40kV, excitation current 50mA;
[0068] Relative crystallinity: measured by Siemens D5005 X-ray diffractometer, with ZSM-5 molecular sieve standard sample of Petrochemical Research Institute as the benchmark (i.e., the relative crystallinity of ZSM-5 molecular sieve standard sample of Petrochemical Research Institute of China Petrochemical Corporation is 100%);
[0069] Specific surface area: determined by using a specific surface area tester based on the N2 adsorption principle and the BET calculation method (see Petrochemical Analysis Method (RIPP Test Method), RIPP151-90, Science Press, published in 1990);
[0070] Pore volume test method: The sample was vacuumed to 1.33×10 at 350°C. -2 Pa, constant temperature and pressure for 15 hours. Tests were conducted at liquid nitrogen temperature of -196°C to measure the adsorption and desorption of N2 under different relative pressures (p / p0). The desorption branch data were calculated using the BJH (Barrett-Joyner-Halenda) method to obtain the pore size distribution data of the sample;
[0071] The transmission electron microscope instrument model is JEM-2100 (200 kV) transmission electron microscope of JEOL Ltd.; the test conditions are: the acceleration voltage is 200 kV, and after the sample is processed, the grain morphology and size of the molecular sieve sample are observed at a magnification of 5000-30000;
[0072] STEM-Mapping test method and instrument: JEOL Ltd. JEM-2100 (200kV) transmission electron microscope. The accelerating voltage of the electron microscope is 200kV. Anhydrous ethanol is dispersed in the sample, and then dripped on the sample net with a diameter of 3mm for observation and testing;
[0073] Test method for the content of metal active components in terms of metal oxides: Semi-quantitative analysis of metal elements is performed by measuring the intensity of characteristic spectral lines of each element through XRF.
[0074] Example 1
[0075] This example uses the following steps to prepare copper-containing ZSM-5 molecular sieve A:
[0076] (1) adding 0.99 g of sodium hydroxide, 40.8 g of deionized water, 20 g of silica gel, 6.78 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.97 g of ZSM-5 seed crystals in sequence under stirring, and stirring well to obtain a first mixture;
[0077] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 55:1:4.68:589; the amount of ZSM-5 seed crystals used is 10 weight % relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0078] (2) dissolving 0.36 g of copper nitrate trihydrate in 10 g of deionized water, adding 0.14 g of sodium persulfate, and stirring thoroughly until a clear and transparent state is obtained to obtain a second mixture;
[0079] The molar ratio of the metal source calculated as CuO, sodium persulfate and the water added in step (2) is 1:0.31:293, and the molar ratio of the aluminum source calculated as Al2O3 and the metal source calculated as CuO is 1:0.285;
[0080] (3) adding the second mixture to the first mixture, mixing thoroughly and then transferring to a stainless steel kettle for hydrothermal treatment at 170° C. for 12 h;
[0081] (4) The product obtained by the hydrothermal treatment in step (3) was filtered, washed to pH=7-8, and ammonium exchanged, dried at 120°C for 12 hours, and then calcined at 550°C for 2 hours in an air atmosphere to obtain a copper-containing ZSM-5 molecular sieve, denoted as A. Its structural parameters are listed in Table 1, its X-ray diffraction spectrum is shown in 1, and its scanning electron microscope photograph is shown in Figure 2 , transmission electron microscopy photos see Figure 3 , Mapping photos see Figure 3 .
[0082] Example 2
[0083] The copper-containing ZSM-5 molecular sieve B was prepared by the same method as in Example 1, except that in step (2), 0.72 g of copper nitrate trihydrate was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the metal source calculated as CuO, sodium persulfate and the water added in step (2) was 1:0.16:293, and the molar ratio of the aluminum source calculated as Al2O3 to the metal source calculated as CuO was 1:0.570. The copper-containing ZSM-5 molecular sieve was prepared and recorded as B, and the structural parameters are listed in Table 1.
[0084] Example 3
[0085] Lanthanum-containing ZSM-5 molecular sieve C was prepared by the same method as in Example 1, except that in step (2), 0.31 g of lanthanum chloride was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the metal source calculated as La2O3, sodium persulfate and the water added in step (2) was 1:0.46:434, and the molar ratio of the aluminum source calculated as Al2O3 to the metal source calculated as La2O3 was 1:0.19. The lanthanum-containing ZSM-5 molecular sieve was obtained, denoted as C, and the structural parameters are listed in Table 1.
[0086] Example 4
[0087] Lanthanum-containing ZSM-5 molecular sieve D was prepared by the same method as in Example 1, except that in step (2), 0.62 g of lanthanum chloride was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the metal source calculated as La2O3, sodium persulfate and the water added in step (2) was 1:0.23:434, and the molar ratio of the aluminum source calculated as Al2O3 to the metal source calculated as La2O3 was 1:0.38. The lanthanum-containing ZSM-5 molecular sieve was obtained, which was denoted as D, and the structural parameters are listed in Table 1.
[0088] Example 5
[0089] The manganese-containing ZSM-5 molecular sieve E was prepared by the same method as in Example 1, except that in step (2), 0.31 g of lanthanum chloride was dissolved in 10 g of deionized water, 0.28 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the metal source calculated as La2O3, sodium persulfate and the water added in step (2) was 1:0.91:428, and the molar ratio of the aluminum source calculated as Al2O3 to the metal source calculated as La2O3 was 1:0.195. The lanthanum-containing ZSM-5 molecular sieve was obtained, which was denoted as E, and the structural parameters are listed in Table 1.
[0090] Example 6
[0091] Nickel-containing ZSM-5 molecular sieve F was prepared by the same method as in Example 1, except that in step (2), 0.2 g of nickel sulfate was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the nickel source calculated as NiO, sodium persulfate and the water added in step (2) was 1:0.78:731, and the molar ratio of the aluminum source calculated as Al2O3 to the nickel source calculated as NiO was 1:0.114. The nickel-containing ZSM-5 molecular sieve was obtained, denoted as F, and its structural parameters are listed in Table 1, its X-ray diffraction spectrum is shown in 8, and its scanning electron microscope photograph is shown in Fig. 9 , transmission electron microscopy photos see Fig.10 , Mapping photos see Fig.11 .
[0092] Example 7
[0093] The nickel-containing ZSM-5 molecular sieve G was prepared by the same method as in Example 1, except that in step (2), 0.5 g of nickel sulfate was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the nickel source calculated as NiO, sodium persulfate and the water added in step (2) was 1:0.31:293, and the molar ratio of the aluminum source calculated as Al2O3 and the nickel source calculated as NiO was 1:0.285. The nickel-containing ZSM-5 molecular sieve was obtained, denoted as G, and its structural parameters are listed in Table 1, its X-ray diffraction spectrum is shown in 12, and its transmission electron microscope photograph is shown in Fig.13 , Mapping photos see Fig.14 .
[0094] Example 8
[0095] The nickel-containing ZSM-5 molecular sieve H was prepared by the same method as in Example 1, except that in step (2), 0.8 g of nickel sulfate was dissolved in 10 g of deionized water, 0.14 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture; wherein the molar ratio of the nickel source calculated as NiO, sodium persulfate and the water added in step (2) was 1:0.2:185, and the molar ratio of the aluminum source calculated as Al2O3 and the nickel source calculated as NiO was 1:0.45. The encapsulated nickel ZSM-5 molecular sieve was obtained, denoted as H, and its structural parameters are listed in Table 1. Its X-ray diffraction spectrum is shown in Fig.15 .
[0096] Example 9
[0097] Nickel-containing ZSM-5 molecular sieve I was prepared by the same method as in Example 1, except that, in step (1), 0.45 g of sodium hydroxide, 38.2 g of deionized water, 20 g of silica gel, 10.08 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.97 g of ZSM-5 seed crystals were added in sequence under stirring, and the mixture was stirred thoroughly to obtain a first mixture; wherein the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide, and water was 37:1:3.15:396; the amount of ZSM-5 seed crystals used was 10 wt% based on the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals was 27, and the average particle size was 1-2 μm;
[0098] In step (2), 0.8 g of nickel sulfate is dissolved in 10 g of deionized water, 0.14 g of sodium persulfate is added, and the mixture is stirred until it is clear and transparent to obtain a second mixture; wherein the molar ratio of the nickel source calculated as NiO, the sodium persulfate and the water added in step (2) is 1:0.2:185, and the molar ratio of the aluminum source calculated as Al2O3 and the nickel source calculated as NiO is 1:0.45. The encapsulated nickel ZSM-5 molecular sieve is obtained, which is denoted as I, and the structural parameters are listed in Table 1.
[0099] Example 10
[0100] The copper-containing ZSM-5 molecular sieve J was prepared by the same method as in Example 1, except that in step (1), 2.92 g of sodium hydroxide, 71.3 g of deionized water, 20 g of silica gel, 4.64 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.28 g of ZSM-5 seed crystals were added in sequence under stirring, and the mixture was stirred well to obtain a first mixture;
[0101] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 80:1:12:1280; the amount of ZSM-5 seed crystals used is 10 wt% relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm. The encapsulated copper ZSM-5 molecular sieve is obtained, denoted as J, and the structural parameters are listed in Table 1.
[0102] Comparative Example 1
[0103] This comparative example illustrates the differences of the metal-free parent ZSM-5 molecular sieve.
[0104] (1) adding 0.99 g of sodium hydroxide, 50.8 g of deionized water, 20 g of silica gel, 6.78 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.97 g of ZSM-5 seed crystals in sequence under stirring, and stirring well to obtain a first mixture; after stirring well, transferring the mixture to a stainless steel kettle, and performing hydrothermal treatment at 170° C. for 12 h;
[0105] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 55:1:4.68:589; the amount of ZSM-5 seed crystals used is 10 weight % relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0106] (2) The product obtained by the hydrothermal treatment in step (1) was filtered, washed to pH = 7-8, and ammonium exchanged, dried at 120°C for 12 hours, and then calcined at 550°C in an air atmosphere for 2 hours to obtain a parent ZSM-5 molecular sieve, denoted as D1, and the structural parameters are listed in Table 1.
[0107] Comparative Example 2
[0108] Nickel-containing ZSM-5 molecular sieve D2 was prepared in the same manner as in Example 6, except that sodium persulfate was not added. Its structural parameters are listed in Table 1.
[0109] Test Case
[0110] The metal-containing ZSM-5 molecular sieves prepared in the examples and comparative examples were subjected to aging treatment. The specific aging treatment method is as follows: the aging furnace is a hydrothermal aging device made by the Institute of Petroleum Science and Technology, and the state after aging at 800°C for 17 hours is used to simulate the balance agent in industrial operation.
[0111] The ZSM-5 molecular sieve prepared in the embodiment and the comparative example was used as a catalyst in the catalytic cracking reaction to carry out the diesel catalytic cracking reaction. The specific method is as follows: the reaction is carried out in a fixed bed reactor, the feed oil is diesel, the carrier gas is nitrogen, the flow rate is 30 mL / min, the reaction temperature is 600°C, the regeneration temperature is 600°C, the reaction pressure is 0.1 MPa, and the weight space velocity is 20 hr -1 The molecular sieve was sieved into 20-40 mesh particles after tableting, the loading amount was 2.0 g, the agent-oil ratio was 1.28, the reaction was 70 s, and the sampling analysis was performed after purging for 900 s, and the material balance calculation was performed. The product distribution is shown in Table 1.
[0112] The following formula is used to calculate the micro-reverse conversion rate X of the raw material and the yield S of the product: i :
[0113]
[0114]
[0115]
[0116]
[0117] Table 1
[0118]
[0119]
[0120]
[0121] According to the data in Table 1, the metal-containing ZSM-5 molecular sieve prepared by the method of introducing a free radical initiator in the present disclosure has a high relative crystallinity of 80-93%. It can be seen from the transmission electron microscopy photos of the metal-containing ZSM-5 molecular sieves prepared in Examples 1 and 6 that the grain size of the metal-containing ZSM-5 molecular sieve prepared by the method of the present disclosure is 1-2 μm; it can be seen from the STEM-Mapping photos of the metal-containing ZSM-5 molecular sieves prepared in Examples 1 and 6 that the metal active components such as Ni, Cu, and La in the metal-containing ZSM-5 molecular sieve prepared by the method of the present disclosure are evenly distributed.
[0122] And according to the data in Table 1, when the metal-containing ZSM-5 molecular sieve prepared by the method disclosed in the present invention is used for diesel catalytic cracking reaction, compared with the metal-free parent molecular sieve, a higher micro-reverse conversion rate and a better low-carbon olefin yield can be obtained; preferably, when the molar ratio of the active metal source, peroxide and water calculated as metal oxide is 1:(0.3-2.7):(250-1200), a higher micro-reverse conversion rate and propylene yield can be obtained; preferably, when the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and water is (35-70):1:(2-10):(350-1000).
[0123] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0124] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0125] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing a metal-containing ZSM-5 molecular sieve, the method comprising: S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture; S2, mixing the active metal source, peroxide, water and the first mixture and performing a hydrothermal reaction; Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent; the metal in the active metal source is one or more of nickel, copper, zinc, manganese, lanthanum and cerium.
2. The method according to claim 1, wherein: Step S2 includes: SS1. Mixing the active metal source, peroxide and water to obtain a second mixture; the molar ratio of the active metal source, peroxide and water in terms of metal oxide is 1:(0.2-3.5):(200-1400), preferably 1:(0.3-2.7):(250-1200); SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as the metal oxide is 1:(0.1-2.0), preferably 1:(0.15-1.5).
3. The method according to claim 1, wherein: In step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (30-100):1:(2-15):(300-1500), preferably (35-70):1:(2-10):(350-1000); Calculated as SiO2, the amount of the seed crystal used is 1-15 wt%, preferably 8-10 wt%, relative to the total weight of the silicon source.
4. The method according to claim 1, wherein: In step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C. and time of 8-32 h.
5. The method according to claim 1, wherein: The method further comprises: subjecting the solid product obtained by the hydrothermal treatment to ammonium exchange and roasting treatment; the conditions of the roasting treatment include: temperature of 400-800° C., time of 0.5-8 hours, and atmosphere of air or water vapor.
6. The method according to claim 1, wherein: The silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; The alkali source includes sodium hydroxide and / or potassium hydroxide; The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm; The active metal source includes one or more of nickel nitrate, nickel sulfate, nickel hydroxide, copper nitrate, copper sulfate, zinc nitrate, zinc sulfate, manganese nitrate, manganese sulfate, lanthanum nitrate, lanthanum sulfate, cerium nitrate and cerium sulfate.
7. The metal-containing ZSM-5 molecular sieve prepared by the method according to any one of claims 1 to 6.
8. The metal-containing ZSM-5 molecular sieve according to claim 7, wherein: The metal-containing ZSM-5 molecular sieve has a structure in which an active metal component is encapsulated inside the ZSM-5 molecular sieve; the active metal component is distributed in the pores of the ZSM-5 molecular sieve.
9. The metal-containing ZSM-5 molecular sieve according to claim 7, wherein: The specific surface area of the metal-containing ZSM-5 molecular sieve is 200-500m 2 / g, with a total pore volume of 0.150-0.22cm 3 ·g -1 , the micropore volume is 0.130-0.180cm 3 ·g -1 , the mesopore volume is 0.010-0.100cm 3 ·g -1 , relative crystallinity is 80-100%; In the metal-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-100; Relative to the total weight of the metal-containing ZSM-5 molecular sieve, the content of the active metal component calculated as metal oxide is 1-3 wt %.
10. Use of the metal-containing ZSM-5 molecular sieve according to any one of claims 7 to 9 in a catalytic cracking reaction of diesel.
11. The use according to claim 10, wherein: The conditions of the catalytic cracking reaction include: a temperature of 530-720°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1-2.
Citation Information
Patent Citations
Boron modified HZSM-5 molecular sieve, preparation method and application thereof
CN106745049A
Fenton reagent modified ZSM-5 molecular sieve catalyst as well as preparation method and application thereof
CN111229304A
Magnesium-containing ZSM-5 shape-selective molecular sieve as well as preparation method and application thereof
CN111760587A
Method for preparing mesoporous ZSM-5 molecular sieve by seed crystal method
CN113912077A
Hierarchical porous Fe / ZSM-5 molecular sieve and preparation method and application thereof