High-purity vanadium pentoxide based on vanadium shale acid leaching solution and preparation method of high-purity vanadium pentoxide

By simplifying the preparation method of vanadium shale acid leaching liquid, combined with countercurrent regular extraction, washing and oxidative back-extraction, the problems of complex processes and environmental pollution in the existing technology are solved, and the low cost and short cycle of high-purity vanadium pentoxide are achieved Preparation and high purity, and improve the vanadium heteroseparation effect.

CN119059558APending Publication Date: 2024-12-03WUHAN UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411089065.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing high-purity vanadium pentoxide preparation process has problems such as complex process, long production cycle, environmental pollution, high chemical consumption and incomplete separation of vanadium miscellaneous.

Method used

Using the preparation method based on the vanadium shale acid leaching solution, the process flow is simplified by adjusting pH, countercurrent regular extraction, washing and oxidative stripping, combining ammonium salt precipitation and roasting steps, hydrogen peroxide and sodium hypochlorite are used as stripping agents to reduce the reverse Extractant dosage and process time.

Benefits of technology

It has achieved high-purity vanadium pentoxide preparation with simple process, low preparation cost, short production cycle and environmentally friendly, with a purity of ≥99.5%, and improved the vanadium heterogeneity separation effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to high-purity vanadium pentoxide based on vanadium shale acid leachate and a preparation method of the high-purity vanadium pentoxide. According to the technical scheme, the method comprises the following steps: adjusting the pH value of an acid leaching solution to 1.8-2.0 to obtain an extraction stock solution; mixing the extraction organic phase with the extraction stock solution, and performing countercurrent positive extraction and phase separation to obtain raffinate and a loaded organic phase; mixing the loaded organic phase with a detergent, performing phase splitting to obtain washing water and a washed loaded organic phase, mixing the washed loaded organic phase with a stripping agent, performing single-stage stripping, and performing phase splitting to obtain a stripping solution and a lean organic phase; adjusting the pH value of the strip liquor to 1.8-2.0 by using dilute sulphuric acid, adding a precipitator, stirring, and carrying out solid-liquid separation to obtain a vanadium precipitation intermediate product and a vanadium precipitation post-liquor; and roasting the vanadium precipitation intermediate product under the condition of 500-550 DEG C to obtain the high-purity vanadium pentoxide based on the vanadium shale acid leaching solution. The method has the characteristics of simple process, environment friendliness and low medicament consumption, and the prepared high-purity vanadium pentoxide based on the vanadium shale acid leachate is high in purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-purity vanadium pentoxide, and specifically relates to high-purity vanadium pentoxide based on vanadium shale acid leaching solution and a preparation method thereof. Background Art

[0002] Vanadium is a strategic resource, widely used in metallurgy, chemical industry, aerospace, energy and other fields. Extracting vanadium pentoxide from vanadium shale has become one of the important ways to obtain vanadium resources. Di(2-ethylhexyl) phosphate (P204) extractant has been maturely used in the industrial production of vanadium solution purification and enrichment. The vanadium-rich solution obtained by extracting vanadium shale stock solution is subjected to oxidation-vanadium precipitation-calcination process to obtain vanadium pentoxide product.

[0003] The patented technology of "Method for preparing vanadium pentoxide from vanadium-containing solution" (CN110317961A) uses sulfur dioxide gas to obtain a reduced vanadium-containing solution, and then obtains vanadium pentoxide by adjusting pH, solid-liquid separation, and calcination. This method eliminates ammonia nitrogen wastewater from the source, but a large amount of sulfuric acid is consumed during the preparation process, and the SO2 gas introduced has a pungent odor, which pollutes the environment. In addition, the purity of the product is more than 98%, and there is still room for improvement in purity and vanadium impurity separation.

[0004] The patented technology of "A method for preparing vanadium pentoxide by vanadium precipitation without ammonium" (CN111020233A) obtains a loaded organic phase and a raffinate by reduction, adjusting the solution pH, and extraction; stripping is performed using hydrogen peroxide and sulfuric acid as stripping agents to obtain a vanadium stripping solution, which is placed for a period of time and then calcined to obtain a vanadium pentoxide product. Although the process of preparing vanadium pentoxide by vanadium precipitation without ammonium proposed in this invention is simple, the concentration of hydrogen peroxide is high and the amount is large during the stripping process, and ammonia water is used to adjust the pH of the vanadium-containing solution, which does not eliminate the environmental impact of ammonia nitrogen wastewater from the source.

[0005] The patented technology of "A method for preparing high-purity vanadium pentoxide" (CN117623383A) is to beat ammonium polyvanadate with water to obtain a mixed slurry; the mixed slurry is heated to 50-80°C, and ammonia water is added to obtain an ammonium polyvanadate solution, and aluminum salt or calcium salt is added under heat preservation conditions for stirring; carbon dioxide gas is continuously introduced to change the solution pH to 6.5-7.5, and solid-liquid separation is performed to obtain an ammonium polyvanadate purified solution; then the temperature is lowered to 10-25°C, crystallization and precipitation are performed, and solid-liquid separation is performed to obtain ammonium metavanadate solid and vanadium precipitation upper layer liquid, which are calcined to obtain a high-purity vanadium pentoxide product. The vanadium pentoxide product obtained by this technology has high purity, but the process is complicated, and the introduced carbon dioxide gas is a greenhouse gas, which pollutes the environment.

[0006] The patented technology of "Method for preparing vanadium pentoxide by reducing vanadium precipitation and vanadium pentoxide and its application" (CN114672668A) uses hydrogen peroxide to strip the organic phase loaded with vanadium to obtain a stripping solution, and then uses a reducing agent to reduce the peroxyvanadate in the stripping solution to polyvanadic acid precipitation, which is then calcined to obtain vanadium pentoxide. Although this technology solves the technical problems of large consumption of sulfuric acid and ammonia water and the output of ammonia nitrogen wastewater during the stripping process, the processing time is relatively long, and the reduction and calcination time is as long as 6 to 12 hours.

[0007] The patented technology of "A method for preparing vanadium pentoxide from vanadium shale extract solution cleanly and without ammonium" (CN115505760A) is to mix the extracted organic phase and the vanadium shale extract solution to obtain the loaded organic phase; then wash and strip to obtain the vanadium-rich solution; adjust its pH value to hydrothermally react at high temperature for 6 to 10 hours, and roast it at 500 to 550℃ in air for 1 to 3 hours to obtain the vanadium pentoxide product. Although this technology has a high vanadium precipitation rate, it takes a long time to react and the process time is long, and the reaction must be carried out in a high temperature environment, which consumes a lot of energy and is not environmentally friendly.

[0008] In summary, the existing preparation of high-purity vanadium pentoxide has problems such as complex process, long production cycle, environmental pollution, high reagent consumption and incomplete separation of vanadium impurities; Summary of the invention

[0009] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution, which has the advantages of simple process, low preparation cost, short production cycle, environmental friendliness and low reagent consumption. The prepared vanadium pentoxide based on vanadium shale acidic leaching solution has high purity.

[0010] To achieve the above purpose, the specific steps of the technical solution adopted by the present invention are:

[0011] Step 1: Adjust pH

[0012] A pH regulator is added to the vanadium shale acid leaching solution to adjust the pH to 1.8-2.0 to obtain an extraction stock solution.

[0013] The composition of the vanadium shale acid leaching solution is: V is 1600-2000 mg / L, Al is 5000-8000 mg / L, Fe is 5000-8000 mg / L, Mg is 1000-3000 mg / L, Na is 1000-3000 mg / L, K is 1000-3000 mg / L, and Ca is 200-500 mg / L.

[0014] The pH of the vanadium shale acidic leaching solution is 0-1.

[0015] Step 2: Extraction and stripping

[0016] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1: (1 to 3), the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 10 to 50° C. The countercurrent extraction stage is 3 to 6, and the countercurrent extraction time is 8 to 12 min. Phase separation is performed to obtain a raffinate and a loaded organic phase.

[0017] The extraction organic phase is a mixture prepared by mixing 15-30 vol% of vanadium extractant, 5 vol% of tributyl phosphate and 65-80 vol% of sulfonated kerosene.

[0018] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:(1-3), the loaded organic phase and the detergent are mixed, stirred at 10-30° C. for 10-40 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0019] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent of (1-4):1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 40-60°C for 8-12 minutes, and the phases are separated to obtain a stripping solution and a lean organic phase.

[0020] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution in a volume ratio of (0.081-0.143) : 1; wherein the mass concentration of the hydrogen peroxide solution is 1.5-6%, and the mass concentration of the sodium hypochlorite solution is 6-10%.

[0021] Step 3: Preparation of vanadium pentoxide

[0022] Step 3.1, adjusting the pH of the stripping solution to 1.8-2.0 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 2-4 times the amount of vanadium in the stripping solution; then stirring at 95-100° C. at a speed of 300-500 r / min for 40-60 min, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation post-liquid.

[0023] Step 3.2: roasting the vanadium precipitation intermediate product at 500-550° C. for 30-60 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0024] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0025] The pH adjuster is sodium hydroxide or sodium bicarbonate.

[0026] The detergent is 0.01-0.05 mol / L dilute sulfuric acid or deionized water.

[0027] The vanadium extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.

[0028] The vanadium concentration in the stripping solution is 15-25 g / L.

[0029] The precipitant is ammonium chloride or ammonium sulfate.

[0030] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is greater than 99.5%.

[0031] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:

[0032] 1. Compared with the existing extraction and chemical precipitation methods for preparing vanadium pentoxide, the present invention proposes a technology for preparing high-purity vanadium pentoxide by acidic leaching solution of vanadium shale - normal extraction - washing - oxidation stripping - ammonium salt vanadium precipitation - roasting. The stripping and oxidation are combined into one step, no irritating gas is introduced, the environment is friendly, the process is shortened, and vanadium precipitation is directly carried out after stripping. The process is simple and the preparation process is short.

[0033] 2. The present invention uses hydrogen peroxide as a stripping agent for oxidative stripping. Compared with the extraction process using sulfuric acid as a stripping agent, pentavalent vanadium oxide and high-valent impurity ions are generated during the stripping process. The high-valent impurity ions have a higher degree of complexation with the organic phase, making it difficult for the impurity ions to fall off from the loaded organic phase; while the vanadium ions are removed from the VO 2+ The structure of vanadium oxyanion oxidized to vanadium is difficult to complex and easier to fall off, thereby improving the selectivity for vanadium, solving the problem of incomplete separation of impurities in the extraction process, and reducing the time of the stripping process, achieving short-time stripping and vanadium extraction, effectively reducing the process time, and achieving good vanadium impurity separation effect. The purity of the obtained high-purity vanadium pentoxide based on vanadium shale acidic leaching solution is ≥99.5%.

[0034] 3. The present invention adopts hydrogen peroxide and sodium hypochlorite for synergistic oxidation, so that hydrogen peroxide still has a high stripping rate under low concentration conditions, reduces the concentration and dosage of hydrogen peroxide during the stripping process, reduces the instability of the stripping agent, reduces the consumption of reagents, and reduces the preparation cost.

[0035] Therefore, the present invention has the characteristics of simple process, low preparation cost, short production cycle, environmental friendliness and low reagent consumption. The high-purity vanadium pentoxide prepared based on vanadium shale acid leaching solution has high purity. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with specific implementation modes, but is not intended to limit the protection scope thereof.

[0037] A high-purity vanadium pentoxide based on vanadium shale acidic leaching solution and a preparation method thereof. The specific steps of the preparation method described in this specific embodiment are:

[0038] Step 1: Adjust pH

[0039] A pH regulator is added to the vanadium shale acid leaching solution to adjust the pH to 1.8-2.0 to obtain an extraction stock solution.

[0040] The composition of the vanadium shale acid leaching solution is: V is 1600-2000 mg / L, Al is 5000-8000 mg / L, Fe is 5000-8000 mg / L, Mg is 1000-3000 mg / L, Na is 1000-3000 mg / L, K is 1000-3000 mg / L, and Ca is 200-500 mg / L.

[0041] The pH of the vanadium shale acidic leaching solution is 0-1.

[0042] Step 2: Extraction and stripping

[0043] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1: (1 to 3), the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 10 to 50° C. The countercurrent extraction stage is 3 to 6, and the countercurrent extraction time is 8 to 12 min. Phase separation is performed to obtain a raffinate and a loaded organic phase.

[0044] The extraction organic phase is a mixture prepared by mixing 15-30 vol% of vanadium extractant, 5 vol% of tributyl phosphate and 65-80 vol% of sulfonated kerosene.

[0045] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:(1-3), the loaded organic phase and the detergent are mixed, stirred at 10-30° C. for 10-40 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0046] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent of (1-4):1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 40-60°C for 8-12 minutes, and the phases are separated to obtain a stripping solution and a lean organic phase.

[0047] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution in a volume ratio of (0.081-0.143) : 1; wherein the mass concentration of the hydrogen peroxide solution is 1.5-6%, and the mass concentration of the sodium hypochlorite solution is 6-10%.

[0048] Step 3: Preparation of vanadium pentoxide

[0049] Step 3.1, adjusting the pH of the stripping solution to 1.8-2.0 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 2-4 times the amount of vanadium in the stripping solution; then stirring at 95-100° C. at a speed of 300-500 r / min for 40-60 min, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation post-liquid.

[0050] Step 3.2: roasting the vanadium precipitation intermediate product at 500-550° C. for 30-60 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0051] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0052] The pH adjuster is sodium hydroxide or sodium bicarbonate.

[0053] The detergent is 0.01-0.05 mol / L dilute sulfuric acid or deionized water.

[0054] The vanadium extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.

[0055] The vanadium concentration in the stripping solution is 15-25 g / L.

[0056] The precipitant is ammonium chloride or ammonium sulfate.

[0057] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is greater than 99.5%.

[0058] Example 1

[0059] A high-purity vanadium pentoxide based on vanadium shale acidic leaching solution and a preparation method thereof. The specific steps of the preparation method described in this embodiment are:

[0060] A pH regulator is added to the vanadium shale acidic leaching solution to adjust the pH to 1.9 to obtain an extraction stock solution.

[0061] The composition of the vanadium shale acid leaching solution is: V is 1998 mg / L; Al is 5010 mg / L; Fe is 6490 mg / L; Mg is 2986 mg / L; Na is 2293 mg / L; K is 1927 mg / L; and Ca is 458.3 mg / L.

[0062] The pH value of the vanadium shale acidic leaching solution is 0.04.

[0063] Step 2: Extraction and stripping

[0064] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1:2, the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 10°C, the countercurrent extraction stage is 6, the countercurrent extraction time is 8 minutes, and the phases are separated to obtain a raffinate and a loaded organic phase.

[0065] The extraction organic phase is a mixture prepared by mixing 15 vol% of a vanadium extractant, 5 vol% of tributyl phosphate and 80 vol% of sulfonated kerosene.

[0066] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:1, the loaded organic phase and the detergent are mixed, stirred at 10° C. for 10 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0067] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent being 1:1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 45° C. The single-stage stripping time is 8 minutes, and the phases are separated to obtain a stripping solution and a lean organic phase.

[0068] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution at a volume ratio of 0.081:1; wherein the mass concentration of the hydrogen peroxide solution is 1.5%, and the mass concentration of the sodium hypochlorite solution is 6%.

[0069] Step 3: Preparation of vanadium pentoxide

[0070] Step 3.1, adjusting the pH of the stripping solution to 1.8 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is twice the amount of the vanadium substance in the stripping solution; then stirring at 95°C and 500 r / min for 45 minutes, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation post-liquid.

[0071] Step 3.2: calcining the vanadium precipitation intermediate product at 500° C. for 45 minutes to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0072] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0073] The pH regulator is sodium hydroxide.

[0074] The detergent is deionized water.

[0075] The vanadium extractant is di(2-ethylhexyl) phosphate.

[0076] The vanadium concentration in the stripping solution is 15 g / L.

[0077] The precipitant is ammonium chloride.

[0078] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is 99.615%.

[0079] Example 2

[0080] A high-purity vanadium pentoxide based on vanadium shale acidic leaching solution and a preparation method thereof. The specific steps of the preparation method described in this embodiment are:

[0081] Step 1: Adjust pH

[0082] A pH regulator is added to the vanadium shale acidic leaching solution to adjust the pH to 2.0 to obtain an extraction stock solution.

[0083] The composition of the vanadium shale acid leaching solution is: V is 1604 mg / L; Al is 7980 mg / L; Fe is 7994 mg / L; Mg is 1534 mg / L; Na is 1002 mg / L; K is 2314 mg / L; and Ca is 324 mg / L.

[0084] The pH value of the vanadium shale acidic leaching solution is 0.4.

[0085] Step 2: Extraction and stripping

[0086] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1:1; the extracted organic phase is mixed with the extracted stock solution, and countercurrent extraction is performed at 25°C, the countercurrent extraction stage is 4, the countercurrent extraction time is 10 minutes, and the phases are separated to obtain a raffinate and a loaded organic phase.

[0087] The extraction organic phase is a mixture prepared by mixing 20 vol% of vanadium extractant, 5 vol% of tributyl phosphate and 75 vol% of sulfonated kerosene.

[0088] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:2, the loaded organic phase and the detergent are mixed, stirred at 20° C. for 20 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0089] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent being 2:1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 40° C. The single-stage stripping time is 10 min, and the phases are separated to obtain a stripping solution and a lean organic phase.

[0090] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution at a volume ratio of 0.09:1; wherein the mass concentration of the hydrogen peroxide solution is 3%, and the mass concentration of the sodium hypochlorite solution is 8%.

[0091] Step 3: Preparation of vanadium pentoxide

[0092] Step 3.1, adjusting the pH of the stripping solution to 2.0 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 2.5 times the amount of vanadium in the stripping solution; then stirring at 100°C and 300 r / min for 50 minutes, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation liquid.

[0093] Step 3.2: calcining the vanadium precipitation intermediate product at 510° C. for 30 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0094] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0095] The pH regulator is sodium bicarbonate.

[0096] The detergent is 0.01 mol / L dilute sulfuric acid.

[0097] The vanadium extractant is 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.

[0098] The vanadium concentration in the stripping solution is 18 g / L.

[0099] The precipitant is ammonium sulfate.

[0100] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is 99.543%.

[0101] Example 3

[0102] A high-purity vanadium pentoxide based on vanadium shale acidic leaching solution and a preparation method thereof. The specific steps of the preparation method described in this embodiment are:

[0103] Step 1: Adjust pH

[0104] A pH regulator is added to the vanadium shale acid leaching solution to adjust the pH to 1.8 to obtain an extraction stock solution.

[0105] The composition of the vanadium shale acid leaching solution is: V is 1735 mg / L; Al is 6535 mg / L; Fe is 5012 mg / L; Mg is 1023 mg / L; Na is 1823 mg / L; K is 1009 mg / L; and Ca is 201 mg / L.

[0106] The pH value of the vanadium shale acidic leaching solution is 0.8.

[0107] Step 2: Extraction and stripping

[0108] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1:3, the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 30°C, the countercurrent extraction stage is 3, the countercurrent extraction time is 12min, and the phases are separated to obtain a raffinate and a loaded organic phase.

[0109] The extraction organic phase is a mixture prepared by mixing 25 vol% of a vanadium extractant, 5 vol% of tributyl phosphate and 70 vol% of sulfonated kerosene.

[0110] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:3, the loaded organic phase and the detergent are mixed, stirred at 25° C. for 30 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0111] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent of 3:1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 50° C. The single-stage stripping time is 12 minutes, and the phases are separated to obtain a stripping solution and a lean organic phase.

[0112] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution at a volume ratio of 0.143:1; wherein the mass concentration of the hydrogen peroxide solution is 4.5%, and the mass concentration of the sodium hypochlorite solution is 10%.

[0113] Step 3: Preparation of vanadium pentoxide

[0114] Step 3.1, adjusting the pH of the stripping solution to 1.9 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 3 times the amount of vanadium in the stripping solution; then stirring at 98°C and 400r / min for 60min, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation liquid.

[0115] Step 3.2: roasting the vanadium precipitation intermediate product at 540° C. for 50 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0116] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0117] The pH regulator is sodium hydroxide.

[0118] The detergent is 0.03 mol / L dilute sulfuric acid.

[0119] The vanadium extractant is di(2-ethylhexyl) phosphate.

[0120] The vanadium concentration in the stripping solution is 22 g / L.

[0121] The precipitant is ammonium chloride.

[0122] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is 99.551%.

[0123] Example 4

[0124] A high-purity vanadium pentoxide based on vanadium shale acidic leaching solution and a preparation method thereof. The specific steps of the preparation method described in this embodiment are:

[0125] Step 1: Adjust pH

[0126] A pH regulator is added to the vanadium shale acidic leaching solution to adjust the pH to 2.0 to obtain an extraction stock solution.

[0127] The composition of the vanadium shale acid leaching solution is: V is 1845 mg / L; Al is 7121 mg / L; Fe is 5941 mg / L; Mg is 2367 mg / L; Na is 2991 mg / L; K is 2996 mg / L; and Ca is 499.4 mg / L.

[0128] The pH of the vanadium shale acidic leaching solution is 1.0.

[0129] Step 2: Extraction and stripping

[0130] Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1:2.5, the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 50°C, the countercurrent extraction stage is 5, the countercurrent extraction time is 9 minutes, and the phases are separated to obtain a raffinate and a loaded organic phase.

[0131] The extraction organic phase is a mixture prepared by mixing 30 vol% of a vanadium extractant, 5 vol% of tributyl phosphate and 65 vol% of sulfonated kerosene.

[0132] Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:2.5, the loaded organic phase and the detergent are mixed, stirred at 30° C. for 40 min, and phase separated to obtain washing water and a washed loaded organic phase.

[0133] Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent being 4:1, the washed loaded organic phase is mixed with the stripping agent, and single-stage stripping is performed at 60° C. The single-stage stripping time is 11 minutes, and phases are separated to obtain a stripping solution and a lean organic phase.

[0134] The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution at a volume ratio of 0.112:1; wherein the mass concentration of the hydrogen peroxide solution is 6%, and the mass concentration of the sodium hypochlorite solution is 9%.

[0135] Step 3: Preparation of vanadium pentoxide

[0136] Step 3.1, adjusting the pH of the stripping solution to 1.8 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 4 times the amount of vanadium in the stripping solution; then stirring at 100°C at a speed of 450r / min for 40min, separating the solid and the liquid, and obtaining a vanadium precipitation intermediate product and a vanadium precipitation post-liquid.

[0137] Step 3.2: calcining the vanadium precipitation intermediate product at 550° C. for 60 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

[0138] The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

[0139] The pH regulator is sodium bicarbonate.

[0140] The detergent is 0.05 mol / L dilute sulfuric acid.

[0141] The vanadium extractant is 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.

[0142] The vanadium concentration in the stripping solution is 25 g / L.

[0143] The precipitant is ammonium sulfate.

[0144] The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is 99.513%.

[0145] Compared with the prior art, this specific implementation has the following positive effects:

[0146] 1. Compared with the existing extraction and chemical precipitation methods for preparing vanadium pentoxide, the proposed vanadium shale acid leaching solution-positive extraction-washing-oxidation stripping-ammonium salt vanadium precipitation-roasting technology for preparing high-purity vanadium pentoxide in this specific embodiment combines stripping and oxidation into one step, does not introduce irritating gases, is environmentally friendly, shortens the process flow, and directly precipitates vanadium after stripping, with a simple process and a short preparation flow.

[0147] 2. This specific embodiment uses hydrogen peroxide as a stripping agent for oxidative stripping. Compared with the extraction process using sulfuric acid as a stripping agent, pentavalent vanadium oxide and high-valent impurity ions are generated during the stripping process. The high-valent impurity ions have a higher degree of complexation with the organic phase, making it difficult for the impurity ions to fall off from the loaded organic phase; while the vanadium ions are removed from the VO 2+ The structure of vanadium oxyanion oxidized to vanadium is difficult to complex and easier to fall off, thereby improving the selectivity for vanadium, solving the problem of incomplete separation of impurities in the extraction process, and reducing the time of the stripping process, achieving short-time stripping and vanadium extraction, effectively reducing the process time, and achieving good vanadium impurity separation effect. The purity of the obtained high-purity vanadium pentoxide based on vanadium shale acidic leaching solution is ≥99.5%.

[0148] 3. This specific embodiment uses hydrogen peroxide and sodium hypochlorite for synergistic oxidation, which achieves a high stripping rate of hydrogen peroxide under low concentration conditions, reduces the concentration and dosage of hydrogen peroxide during the stripping process, reduces the instability of the stripping agent, reduces the consumption of reagents, and reduces the preparation cost.

[0149] Therefore, the specific implementation method has the characteristics of simple process, low preparation cost, short production cycle, environmental friendliness and low reagent consumption, and the high-purity vanadium pentoxide prepared based on vanadium shale acid leaching solution has high purity.

Claims

1. A method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution, characterized in that The specific steps of the preparation method are: Step 1: Adjust pH Adding a pH regulator to the vanadium shale acidic leaching solution to adjust the pH to 1.8-2.0 to obtain an extraction stock solution; The composition of the vanadium shale acidic leaching solution is: V is 1600-2000 mg / L, Al is 5000-8000 mg / L, Fe is 5000-8000 mg / L, Mg is 1000-3000 mg / L, Na is 1000-3000 mg / L, K is 1000-3000 mg / L, and Ca is 200-500 mg / L; The pH of the vanadium shale acidic leaching solution is 0-1; Step 2: Extraction and stripping Step 2.1, according to the volume ratio of the extracted organic phase to the extracted stock solution of 1: (1-3), the extracted organic phase and the extracted stock solution are mixed, and countercurrent extraction is performed at 10-50° C., the countercurrent extraction stage is 3-6 stages, the countercurrent extraction time is 8-12 min, and phase separation is performed to obtain a raffinate and a loaded organic phase; The extraction organic phase is a mixture prepared by mixing 15-30 vol% of a vanadium extractant, 5 vol% of tributyl phosphate and 65-80 vol% of sulfonated kerosene; Step 2.2, according to the volume ratio of the loaded organic phase to the detergent being 1:(1-3), the loaded organic phase and the detergent are mixed, stirred at 10-30° C. for 10-40 min, and phase separated to obtain washing water and a washed loaded organic phase; Step 2.3, according to the volume ratio of the washed loaded organic phase to the stripping agent being (1-4):1, the washed loaded organic phase and the stripping agent are mixed, and single-stage stripping is performed at 40-60° C. The single-stage stripping time is 8-12 min, and phases are separated to obtain a stripping solution and a lean organic phase; The stripping agent is a mixture prepared by mixing the sodium hypochlorite solution and the hydrogen peroxide solution in a volume ratio of sodium hypochlorite solution to hydrogen peroxide solution of (0.081-0.143):1; wherein the mass concentration of the hydrogen peroxide solution is 1.5-6%, and the mass concentration of the sodium hypochlorite solution is 6-10%; Step 3: Preparation of vanadium pentoxide Step 3.1, adjusting the pH of the stripping solution to 1.8-2.0 with 3% by volume dilute sulfuric acid, and then adding a precipitant, wherein the amount of the precipitant added is 2-4 times the amount of vanadium in the stripping solution; then stirring at 95-100° C. at a speed of 300-500 r / min for 40-60 min, and separating the solid and liquid to obtain a vanadium precipitation intermediate product and a vanadium precipitation liquid; Step 3.2: calcining the vanadium precipitation intermediate product at 500-550° C. for 30-60 min to obtain high-purity vanadium pentoxide based on vanadium shale acid leaching solution.

2. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The valence state of vanadium in the vanadium shale acidic leaching solution is tetravalent, and the valence state of iron is divalent.

3. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The pH adjuster is sodium hydroxide or sodium bicarbonate.

4. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The detergent is 0.01-0.05 mol / L dilute sulfuric acid or deionized water.

5. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The vanadium extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono(2-ethylhexyl) ester.

6. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The vanadium concentration in the stripping solution is 15-25 g / L.

7. The method for preparing high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to claim 1, characterized in that The precipitant is ammonium chloride or ammonium sulfate.

8. A high-purity vanadium pentoxide based on vanadium shale acid leaching solution, characterized in that The high-purity vanadium pentoxide based on vanadium shale acidic leaching solution is prepared by the preparation method of high-purity vanadium pentoxide based on vanadium shale acidic leaching solution according to any one of claims 1 to 7; The purity of the high-purity vanadium pentoxide based on the vanadium shale acidic leaching solution is greater than 99.5%.

Citation Information

Cited By

  • Method for preparing vanadium pentoxide by using high-acidity vanadium-containing solution

    CN119929876A

  • A method for preparing vanadium pentoxide using a high-acidity vanadium-containing solution