Aluminum oxide-zirconium oxide composite powder as well as preparation method and application thereof
By introducing magnesium oxide, calcium oxide and silica as additives, and using wet grinding process to treat alumina and zirconia, the problem of uneven particle size of alumina-zirconia composite ceramic powder is solved, and the ceramics is significantly improved Hardness, strength and toughness, and maintain good performance at high temperatures.
Patent Information
- Application Number
- CN202411292237.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The particle size of the existing alumina-zirconia composite ceramic powder is uneven, which leads to local eutectic melting and stress concentration during ceramic sintering, resulting in problems of degraded mechanical properties and low yield.
By introducing magnesium oxide, calcium oxide and silica as additives, and using wet grinding process, alumina and zirconia are processed separately, the grinding media and process parameters are optimized, and alumina-zirconia composite powder with uniform size and uniformity is obtained. The material is then molded and sintered.
The prepared alumina-zirconia composite ceramic has significantly improved hardness, strength and toughness, and is higher in hardness than pure alumina ceramics, and exhibits good durability and stability at high temperatures, which are suitable for high-temperature working conditions.
Smart Images

Figure CN119059800A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials, and in particular to an alumina-zirconium oxide composite powder and a preparation method and application thereof. Background Art
[0002] Ceramic materials have been widely used in machinery, electronics, chemical industry, aerospace and other fields due to their excellent properties such as high hardness, high wear resistance, high temperature resistance and corrosion resistance. Alumina ceramics and zirconia ceramics are two common ceramic materials, each with unique performance advantages. Alumina ceramics have the advantages of high hardness, high strength, high wear resistance, high temperature resistance and corrosion resistance, but its toughness is relatively low. Zirconia ceramics have the advantages of high toughness, high strength, high temperature resistance and corrosion resistance, but its hardness is relatively low. With the demand for ceramics with both high toughness and high hardness in medical equipment, electronic equipment, automobile manufacturing, aerospace, tool manufacturing, industrial machinery and other fields, researchers intend to use the performance advantages of alumina ceramics and zirconia ceramics to obtain ceramics with both high toughness and high hardness by compounding alumina and zirconia.
[0003] At present, the alumina-zirconia composite powder required for the preparation of alumina-zirconia composite ceramics is usually obtained by adding additives or other components to the processed alumina powder and then grinding and mixing it twice. However, due to the large difference in particle size of different powders and the great difference in dispersion ability, the powder obtained by this mixing method has poor uniformity, especially for larger agglomerated particles, which will lead to local eutectic melting and other states during ceramic sintering, causing local stress, resulting in defects in the ceramic, reduced mechanical properties, etc., and low yield rate. Therefore, there is an urgent need for a preparation method for alumina-zirconia composite powders with uniform size and good uniformity to improve the performance of alumina-zirconia composite ceramics prepared therefrom. Summary of the invention
[0004] The present invention provides an alumina-zirconia composite powder and a preparation method and application thereof. The present invention obtains an alumina-zirconia composite powder with uniform size and good powder uniformity by introducing specific additives and improving the preparation process. The alumina-zirconia composite ceramic prepared from the alumina-zirconia composite powder has high strength, high toughness and good high temperature resistance, and its hardness is higher than that of pure alumina ceramics.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A first aspect of the present invention provides an alumina-zirconia composite powder comprising the following components in mass percentage: 60wt%-70wt% of alumina, 20wt%-35wt% of zirconium oxide and 1.5wt%-5wt% of additives, wherein the additives include magnesium oxide, calcium oxide and silicon dioxide.
[0007] The second aspect of the present invention provides a method for preparing the alumina-zirconia composite powder according to the first aspect, comprising the following steps:
[0008] (1) performing a first wet grinding of micron-sized aluminum oxide and a micron-sized first additive in the presence of water to obtain a first slurry; the micron-sized first additive comprises micron-sized magnesium oxide and micron-sized silicon dioxide; and the D50 of the particles in the first slurry is less than 300 nm;
[0009] Performing a second wet grinding of the micron-sized zirconium oxide and the micron-sized second additive in the presence of water to obtain a second slurry; the micron-sized second additive comprises micron-sized magnesium oxide and micron-sized calcium oxide; the D50 of the particles in the second slurry is less than 500 nm;
[0010] (2) The first slurry and the second slurry are stirred and mixed evenly, and dried to obtain the alumina-zirconia composite powder.
[0011] Furthermore, in step (1), before wet grinding, each raw material is first crushed and ground to a micron-sized particle size for better dispersion and to obtain a more uniformly mixed powder; preferably, the particle size of the micron-sized aluminum oxide is preferably 0.2-0.5 μm; the particle size of the micron-sized magnesium oxide is preferably 1-2 μm; the particle size of the micron-sized silicon dioxide is preferably 2-5 μm; the particle size of the micron-sized zirconium oxide is preferably 0.4-0.6 μm; and the particle size of the micron-sized calcium oxide is preferably 1-2 μm.
[0012] Furthermore, in step (1), the mass ratio of micron-sized magnesium oxide to micron-sized silicon dioxide in the micron-sized first additive is preferably 3:2; and the mass ratio of micron-sized magnesium oxide to micron-sized calcium oxide in the micron-sized second additive is preferably 2:1.
[0013] Furthermore, in step (1), micron-sized alumina is first dispersed in water to obtain an alumina dispersion, and then a micron-sized first additive is added to perform a first wet grinding; preferably, the solid content of the alumina dispersion is 30%-50%, and the mass ratio of the micron-sized first additive to the micron-sized alumina is (0.02-0.05):1.
[0014] Furthermore, in step (1), micron-sized zirconium oxide is first dispersed in water to obtain a zirconium oxide dispersion, and then a micron-sized second additive is added to perform a second wet grinding; preferably, the solid content of the zirconium oxide dispersion is 20%-40%; and the mass ratio of the micron-sized second additive to the micron-sized zirconium oxide is (0.01-0.03):1.
[0015] Furthermore, in step (1), in the first wet grinding step: the grinding medium is 0.2-0.5 mm zirconium oxide grinding beads, the ball-to-material ratio is (4-6): 1, grinding is 4-6 hours, and the grinding speed is 1600-2200 rpm; preferably, the grinding speed is set to increase during the first wet grinding process. In some preferred embodiments, the ball-to-material ratio is 5:1, and the first wet grinding treatment is carried out according to grinding at 1600 rpm for 1 hour, grinding at 1800 rpm for 1 hour, grinding at 2000 rpm for 1 hour, and grinding at 2200 rpm for 2 hours.
[0016] Furthermore, in step (2), in the step of the second wet grinding, the grinding medium is 0.2-0.5 mm zirconium oxide grinding beads, the ball-to-material ratio is (4-6): 1, grinding is 5-7 hours, and the grinding speed is 1800-2400 rpm; preferably, the grinding speed is set to increase during the second wet grinding process. In some preferred embodiments, the ball-to-material ratio is 5:1, and the second wet grinding process is carried out according to grinding at 1800 rpm for 1 hour, grinding at 2000 rpm for 1 hour, grinding at 2200 rpm for 2 hours, and grinding at 2000 rpm for 2 hours.
[0017] Furthermore, in step (2), the stirring time is preferably 1-3 h, such as 1 h, 2 h, 3 h, etc.
[0018] Furthermore, in step (2), the drying temperature is preferably 100-110°C.
[0019] The third aspect of the present invention provides an alumina-zirconia composite ceramic, which is prepared from the alumina-zirconia composite powder described in the first aspect or the alumina-zirconia composite powder described in the second aspect.
[0020] Furthermore, the alumina-zirconia composite powder is subjected to a molding process and then sintered in an inert atmosphere to obtain the alumina-zirconia composite ceramic; the molding process includes dry pressing, isostatic pressing, injection molding, etc., and in the dry pressing step: the pressure is 80-120MPa, and the holding time is 5-10min; the sintering temperature is 1300-1400°C, and the sintering time is 3-6h, for example, sintering at 1350°C for 4h.
[0021] Furthermore, the hardness of the alumina-zirconia composite powder is greater than 1500 HV.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention provides an alumina-zirconia composite powder and a preparation method thereof, wherein alumina and zirconia are processed separately by wet grinding, and magnesium oxide and silicon dioxide are introduced during the wet grinding of alumina, and magnesium oxide and calcium oxide are introduced during the wet grinding of zirconia, and the alumina-zirconia composite powder with uniform size and good powder uniformity is obtained in combination with the above-mentioned grinding process in the presence of the above-mentioned specific additives. The above-mentioned preparation method is simple to operate and has good process controllability, and is suitable for mass production of alumina-zirconia composite powder.
[0024] 2. The alumina-zirconia composite ceramics prepared by the alumina-zirconia composite powder prepared by the present invention have extremely high hardness, and the hardness is significantly improved compared with the traditional single alumina ceramics or zirconia ceramics. According to the Vickers hardness tester, under the conditions of a loading force of 50N and a loading time of 15s, the hardness of the alumina-zirconia composite ceramic material of the present invention can reach 1800HV, which is much higher than the hardness of pure alumina ceramics (hardness of 1500HV) and pure zirconia ceramics (hardness of 1200HV) under the same test conditions. In addition, the alumina-zirconia composite ceramics prepared by the present invention also have excellent strength performance (bending strength can reach 800MPa), toughness (fracture toughness can reach 8MPa·m^(1 / 2)) and high temperature resistance, etc. When subjected to external force, it is not easy to break and damage, and can effectively absorb impact capacity, ensuring the reliability of the material during use, and can be used for a long time at a high temperature of 1500°C without obvious performance degradation, and is suitable for applications under high temperature working conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a picture of the alumina-zirconia composite powder prepared in Example 1. DETAILED DESCRIPTION
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The term "includes" or "comprising" described in the present invention means that it may include or contain other components in addition to the components described. The term "includes" or "comprising" described in the present invention may also be replaced by the closed form "for" or "consisting of..."
[0027] The present invention is further described below in conjunction with specific embodiments and drawings so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0028] Example 1
[0029] This embodiment relates to the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic, wherein the alumina-zirconia composite powder comprises 70% alumina, 25% zirconium oxide, 3.1% magnesium oxide, 0.5% calcium oxide and 1.4% silicon dioxide, as follows:
[0030] Preparation of alumina-zirconia composite powder:
[0031] (1) A certain amount of magnesium oxide, calcium oxide, silicon dioxide and other additives are put into a planetary ball mill in batches for grinding and crushing. The grinding beads are zirconium oxide beads with particle sizes of 5 mm, 3 mm and 1 mm, respectively, and the mass ratio of the grinding balls is 1:2:2. The rotation speed is 400 rpm. The ball milling time is adjusted according to the required particle size after refinement. The particle size requirements of the additives after grinding are as follows: magnesium oxide D50 is 1 μm and 1.5 μm, calcium oxide D50 is 1 μm, and silicon dioxide D50 is 2 μm.
[0032] (2) Alumina powder is added to water to prepare alumina slurry with a solid content of 40%, and then additives are added. The additives are magnesium oxide (1.5μm) and silicon dioxide (2μm) in a mass ratio of 3:2. The amount of additives added is 3.5% of the alumina powder, of which magnesium oxide is 2.1% and silicon dioxide is 1.4%. The above materials are mixed and compounded and added to a horizontal sand mill for wet sand grinding. The ball-to-material ratio of the sand mill is 5:1, and the particle size of the zirconium oxide medium grinding beads is 0.2-0.5mm. The sand mill speed is gradually adjusted according to 1600rpm 1h, 1800rpm 1h, 2000rpm 1h, and 2200rpm 2h. Grind for 5 hours to make the alumina D50 reach below 300nm. The mixed slurry after wet grinding obtains slurry 1.
[0033] (3) Add water to the zirconium oxide powder to prepare an alumina slurry with a solid content of 30%, and then add additives. The additives are magnesium oxide (1 μm) and calcium oxide (1 μm) in a mass ratio of 2:1. The amount of additives added is 1.5% of the alumina powder, of which magnesium oxide is 1% and silicon dioxide is 0.5%. After the above materials are mixed and compounded, they are added to a horizontal sand mill for wet sand grinding. The ball-to-material ratio of the sand mill is 5:1, and the particle size of the zirconium oxide medium grinding beads is 0.2-0.5mm. The sand mill speed is gradually adjusted according to 1800rpm 1h, 2000rpm 1h, 2200rpm2h, and 2400rpm 2h. Grind for 6 hours to make the alumina D50 reach below 500nm. The mixed slurry after wet grinding obtains slurry 2.
[0034] (4) Slurry 1 and slurry 1 are added in a constant temperature stirrer at a certain mass ratio of 2:1 and stirred for 1 hour, and then dried in an oven at 100-110°C for 4 hours to obtain an alumina-zirconia composite powder, such as Figure 1 shown.
[0035] Preparation of alumina-zirconia composite ceramics:
[0036] The above-mentioned alumina-zirconia composite powder is loaded into a mold and dry-pressed. The molding pressure is 100 MPa and the holding time is 10 minutes. The formed body is placed in a sintering furnace and sintered at 1350°C for 4 hours in a nitrogen atmosphere to obtain an alumina-zirconia composite ceramic.
[0037] Example 2
[0038] The present embodiment relates to the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic. The only difference from Example 1 is that the alumina-zirconia composite powder contains 65% alumina, 30% zirconium oxide, 3.1% magnesium oxide, 0.5% calcium oxide and 1.4% silicon dioxide. The remaining operations are the same to prepare the corresponding alumina-zirconia composite powder and alumina-zirconia composite ceramic.
[0039] Example 3
[0040] The present embodiment relates to the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic. The only difference from Example 1 is that the alumina-zirconia composite powder contains 60% alumina, 35% zirconium oxide, 3.1% magnesium oxide, 0.5% calcium oxide and 1.4% silicon dioxide. The remaining operations are the same to prepare the corresponding alumina-zirconia composite powder and alumina-zirconia composite ceramic.
[0041] Comparative Example 1
[0042] This comparative example involves the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic, and the only difference from Example 1 is that the alumina-zirconia composite powder contains 70% alumina, 25% zirconium oxide, and 5% magnesium oxide, wherein an equal amount of magnesium oxide is used to replace silicon dioxide and calcium oxide, and the other operations are the same, to prepare the corresponding alumina-zirconia composite powder and alumina-zirconia composite ceramic.
[0043] Comparative Example 2
[0044] This comparative example involves the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic. The only difference from Example 1 is that the order of adding silicon dioxide and calcium oxide is changed, and the other operations are the same to prepare the corresponding alumina-zirconia composite powder and alumina-zirconia composite ceramic.
[0045] Comparative Example 3
[0046] This comparative example relates to the preparation of an alumina-zirconia composite powder and an alumina-zirconia composite ceramic, which is different from Example 1 only in that all materials are mixed once and crushed by wet sand milling, wherein the ball-to-material ratio of the sand milling is 5:1, and the particle size of the zirconium oxide medium grinding beads is 0.2-0.5 mm. The sand milling speed is gradually adjusted according to 1800rpm 1h, 2000rpm 1h, 2200rpm2h, and 2400rpm 2h, and the mixed slurry is obtained by grinding for 6 hours, and dried in an oven at 100-110°C for 4 hours to obtain an alumina-zirconia composite powder.
[0047] Preparation of alumina-zirconia composite ceramics:
[0048] The above-mentioned alumina-zirconia composite powder is loaded into a mold and dry-pressed. The molding pressure is 100 MPa and the holding time is 10 minutes. The formed body is placed in a sintering furnace and sintered at 1350°C for 4 hours in a nitrogen atmosphere to obtain an alumina-zirconia composite ceramic.
[0049] Comparative Example 4
[0050] This comparative example involves the preparation of a pure alumina ceramic, which differs from Example 1 only in that a pure alumina ceramic powder contains 95% alumina, 3.1% magnesium oxide, 0.5% calcium oxide and 1.4% silicon dioxide, and the remaining operations are the same to prepare the corresponding pure alumina ceramic.
[0051] Comparative Example 5
[0052] This comparative example involves the preparation of a pure zirconia ceramic, which differs from Example 1 only in that a pure alumina ceramic powder contains 95% zirconium oxide, 3.1% magnesium oxide, 0.5% calcium oxide and 1.4% silicon dioxide, and the remaining operations are the same to prepare the corresponding pure zirconia ceramic.
[0053] Performance Testing
[0054] The hardness, three-point bending strength, fracture toughness and high temperature resistance of the alumina-zirconia composite ceramics prepared in the above Examples 1-3 and Comparative Examples 1-3, the pure alumina ceramics prepared in Comparative Example 4 and the pure zirconia ceramics prepared in Comparative Example 5 were tested. The test method is as follows:
[0055] Hardness test: Use a diamond indenter with a cone angle of 120 degrees and a top spherical radius of 0.2mm. Press the indenter into the material surface with a rated test force (50N) for a rated time (15s). Then remove the test force and obtain the hardness value based on the depth of the indentation.
[0056] Three-point bending strength test: Use a measuring tool with an accuracy of 0.01mm, such as a vernier caliper or micrometer, to measure the length, width, thickness and other dimensions of the specimen, and record the measured values of each specimen. Place the specimen horizontally on the two supporting cylinders of the three-point bending fixture, ensuring that the long axis of the specimen is perpendicular to the loading direction and the center of the specimen is located at the midpoint of the two supporting cylinders. According to the test requirements and the characteristics of the ceramic material, set the loading speed of the testing machine and the data acquisition frequency of the testing machine to accurately record the load and displacement data during the test. Start the testing machine and move the loading cylinder downward at the set speed to apply a vertical load to the specimen. During the test, closely observe the deformation of the specimen until the specimen breaks. The testing machine automatically records the maximum load when the specimen breaks and the corresponding displacement and other data. For each specimen, its breaking load value must be recorded. The three-point bending strength (σ) of the ceramic is calculated according to the formula σ=3FL / 2bh2, in megapascals (MPa); where F is the maximum load when the specimen breaks (N), L is the span between the centers of the two supporting cylinders, i.e., the span (mm), b is the width of the specimen (mm), and h is the thickness of the specimen (mm).
[0057] Fracture toughness test: Use an indenter to apply a certain load on the smooth ceramic surface until obvious cracks appear at the four corners of the indentation. Use an optical or scanning electron microscope to measure the indentation size and the length of the crack, and calculate the fracture toughness value of the material by combining the load, material hardness and elastic modulus, and calibration constants.
[0058] High temperature resistance test: Place the ceramic sample directly into a high temperature furnace and heat it at different set temperatures. At each temperature stage, observe the appearance changes of the ceramic sample, such as color change, cracks, deformation, etc. At the same time, you can use measuring tools (such as calipers) to measure the size change of the sample, judge its dimensional stability, and determine its high temperature resistance.
[0059] The test results are shown in Table 1 below:
[0060] Table 1
[0061]
[0062] It can be seen from Table 1 that the alumina-zirconia composite ceramics prepared in Examples 1-3 have higher strength, toughness and better high temperature resistance than pure alumina ceramics (Comparative Example 4) and pure zirconia ceramics (Comparative Example 5). Among them, the hardness of the alumina-zirconia composite ceramics prepared in Example 1 can be as high as 1800HV (better than pure alumina ceramics), the bending strength is as high as 800MPa, the fracture toughness is much better than pure zirconia ceramics, up to 8MPa·m^(1 / 2), and has excellent stability below 1550℃.
[0063] It can be seen from Example 1 and Comparative Examples 1 and 2 that the introduction and order of addition of silicon dioxide and calcium oxide will affect the hardness, strength, toughness, etc. of the composite ceramic; in addition, in Comparative Example 3, the materials are directly mixed once and wet sand milled to prepare the composite powder, and the hardness of the composite ceramic prepared therefrom is greatly reduced, which is less than the hardness of pure alumina ceramics, and other properties are also significantly reduced compared with Example 1. It can be seen that the present invention can effectively improve the uniformity of each component in the powder and the mechanical properties of the ceramic after sintering by improving the powder composition and preparation process.
[0064] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. An alumina-zirconia composite powder, characterized in that: The invention comprises the following components in mass percentage: 60wt%-70wt% of aluminum oxide, 20wt%-35wt% of zirconium oxide and 1.5wt%-5wt% of additives, wherein the additives comprise magnesium oxide, calcium oxide and silicon dioxide.
2. A method for preparing the alumina-zirconia composite powder according to claim 1, characterized in that: The following steps are involved: (1) performing a first wet grinding of micron-sized aluminum oxide and a micron-sized first additive in the presence of water to obtain a first slurry; the micron-sized first additive comprises micron-sized magnesium oxide and micron-sized silicon dioxide; and the D50 of the particles in the first slurry is less than 300 nm; Performing a second wet grinding of the micron-sized zirconium oxide and the micron-sized second additive in the presence of water to obtain a second slurry; the micron-sized second additive comprises micron-sized magnesium oxide and micron-sized calcium oxide; the D50 of the particles in the second slurry is less than 500 nm; (2) The first slurry and the second slurry are stirred and mixed evenly, and dried to obtain the alumina-zirconia composite powder.
3. The preparation method according to claim 2, characterized in that: In step (1), the particle size of the micron-sized aluminum oxide is 0.2-0.5 μm; The particle size of the micron-sized magnesium oxide is 1-2 μm; The particle size of the micron-sized silicon dioxide is 2-5 μm; The particle size of the micron-sized zirconium oxide is 0.4-0.6 μm; The particle size of the micron-sized calcium oxide is 1-2 μm.
4. The preparation method according to claim 2, characterized in that: In step (1), the mass ratio of micron-sized magnesium oxide to micron-sized silicon dioxide in the micron-sized first additive is 3:2; The mass ratio of micron-sized magnesium oxide to micron-sized calcium oxide in the micron-sized second additive is 2:
1.
5. The preparation method according to claim 2, characterized in that: In step (1), micron-sized aluminum oxide is first dispersed in water to obtain an aluminum oxide dispersion, and then a micron-sized first additive is added to perform a first wet grinding; The solid content of the aluminum oxide dispersion is 30%-50%; The mass ratio of the micron-sized first additive to the micron-sized aluminum oxide is (0.02-0.05):
1.
6. The preparation method according to claim 2, characterized in that: In step (1), the micron-sized zirconium oxide is first dispersed in water to obtain a zirconium oxide dispersion, and then a micron-sized second additive is added to perform a second wet grinding; The solid content of the zirconium oxide dispersion is 20%-40%; The mass ratio of the micron-sized second additive to the micron-sized zirconium oxide is (0.01-0.03):
1.
7. The preparation method according to claim 2, characterized in that: In step (1), in the first wet grinding step: the grinding medium is 0.2-0.5 mm zirconium oxide grinding beads, the ball-to-material ratio is (4-6): 1, grinding is 4-6 hours, and the grinding speed is 1600-2200 rpm; preferably, the grinding speed is set to increase during the first wet grinding process; In the second wet grinding step: the grinding medium is 0.2-0.5mm zirconium oxide grinding beads, the ball-to-material ratio is (4-6):1, grinding is 5-7h, and the grinding speed is 1800-2400rpm; preferably, the grinding speed is set to increase during the second wet grinding process.
8. The preparation method according to claim 2, characterized in that: In step (2), the stirring time is 1-3 hours; The drying temperature is 100-110°C.
9. An alumina-zirconia composite ceramic, characterized in that: The composite powder is prepared from the alumina-zirconia composite powder according to claim 1 or the alumina-zirconia composite powder according to any one of claims 2 to 8.
10. The alumina-zirconia composite ceramic according to claim 9, characterized in that: The alumina-zirconia composite powder is molded and then sintered in an inert atmosphere to obtain the alumina-zirconia composite ceramic; The molding process includes dry pressing molding, wherein the pressure is 80-120 MPa and the holding time is 5-10 min; The sintering temperature is 1300-1400° C., and the sintering time is 3-6 hours.
Citation Information
Patent Citations
Preparation method for self-complement sub-micron crystal alumina ceramic
CN101343176A
Ceramic slurry of submicron powder with high solid content, low viscosity and high dispersity and preparation method thereof
CN101941834A
Aluminum oxide ceramic composite material as well as preparation method and application thereof
CN113860857A
Preparation method of ceramic powder and process for preparing ceramic nozzle by using powder
CN116354707A
Alumina-zirconia-based ceramic and production method therefor
JP2005239469A