Acrylate polymer microsphere, preparation method and application thereof, and system for preparing acrylate polymer microsphere

Through step-by-step polymerization and control of the reaction heat, the problems of large particle size and uneven dispersion of polymer microspheres in traditional methods were solved, and acrylate polymer microspheres with suitable particle size and small dispersion coefficient were prepared, and the polyolefins were used to prepare the polyolefins. The haze effect is significantly improved when applied in films.

CN119060227AActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310623413.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

In the traditional preparation method of acrylate polymer microspheres, heat transfer in the reaction system is difficult to control, resulting in large particle size and uneven dispersion, wide molecular weight distribution, affecting product quality.

Method used

Step-by-step polymerization method is adopted, and by controlling the conversion rate of each step of polymerized monomer within a specific range, combining stirring and nitrogen bubble technology, ensuring easy management of reaction heat, and using insoluble dispersion media to prepare suitable particle size , microspheres with small dispersion coefficient and narrow molecular weight distribution.

Benefits of technology

The uniformity of polymer microspheres is improved, the particle size is suitable, the dispersion coefficient is small, the molecular weight distribution is narrow, and a high haze effect is obtained when used as a modifier in a polyolefin film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060227A_ABST
    Figure CN119060227A_ABST
Patent Text Reader

Abstract

The invention relates to the field of polymer synthesis, and relates to an acrylate polymer microsphere, a preparation method and application thereof, and a system for preparing the acrylate polymer microsphere. Comprising the following steps: S1, uniformly mixing a dispersion medium, a stabilizer, an initiator and a monomer to obtain a first mixture; s2, performing step-by-step polymerization on the first mixture to obtain a second mixture; s3, separating the second mixture to obtain acrylate polymer microspheres; the dispersion medium and the monomer are immiscible; the step-by-step polymerization is N-step polymerization, and N is greater than or equal to 2; the monomer conversion rate of the Nth step is 1-5 times of the monomer conversion rate of the (N-1) th step; according to the method, the polymerization reaction is carried out step by step, so that heat transfer of a polymerization reaction system is easier to control, reaction heat is further removed, and the uniformity of the polymer microspheres is improved. Meanwhile, the dispersion medium and the monomer are immiscible, so that the prepared polymer microspheres have the characteristics of proper particle size, small dispersion coefficient and narrow molecular weight distribution index.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer synthesis, and in particular to an acrylate polymer microsphere, a preparation method and application thereof, and a system for preparing the acrylate polymer microsphere. Background Art

[0002] Usually, the dispersion polymerization of acrylic acid ester monomers is carried out in a kettle reactor, while under laboratory conditions, ordinary glass bottles are commonly used reaction containers, such as Yu Xianglin et al., Preparation of monodisperse micron-sized cross-linked polymethyl methacrylate microspheres by alcohol-water dispersion polymerization, Journal of Hubei University (Natural Science Edition) 2003, 25(2): 137-140. Men Shumei et al., Preparation of monodisperse polymethyl methacrylate microspheres, Liaoning Chemical Industry, 2012, 41(12): 1242-1244. Jiang Xueliang et al., Study on the preparation process of monodisperse narrow distribution PMMA microspheres, Journal of Hubei University (Natural Science Edition) 2014, 36(2): 138-142. The polymer microspheres obtained above are at the micron level, but the molecular weight distribution is usually wide.

[0003] Recently, there are also non-traditional processes for preparing polymethyl methacrylate microspheres. The oil phase fluid forms a jet through the nozzle, and the oil phase jet is dispersed in the water phase under vibration to form uniform droplets. The uniform oil droplets enter the fluidized reactor and polymerize to obtain monodisperse polymethyl methacrylate microspheres. The microspheres are relatively large, with an average particle size of about 350 microns, for example, Wang Ye et al., Preparation and properties of monodisperse polymethyl methacrylate magnetic microspheres, Chemical Engineering, 2015, 43(9): 40-44.

[0004] In traditional reaction processes, since heat transfer in the reaction system is difficult to control, it has some impact on the final quality of the polymer product, such as larger polymer particle size, uneven particle size dispersion, and wider polymer molecular weight distribution. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the heat transfer of the reaction system is difficult to control and the preparation method is complicated in the prior art, resulting in a large particle size of polymer microspheres and uneven particle size. An acrylate polymer microsphere and its preparation method and application, and a system for preparing acrylate polymer microspheres are provided. In the preparation method, the polymerization reaction is carried out step by step, and the conversion rate of each step of the polymerization monomer is controlled to meet a specific range, so that the reaction heat in the reaction process can be easily removed and the uniformity of the polymer microspheres can be improved. At the same time, the dispersion medium and the monomer are immiscible with each other, and the prepared polymer microspheres have the characteristics of suitable particle size, small dispersion coefficient, and narrow molecular weight distribution index.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing acrylic polymer microspheres, characterized in that the method comprises the following steps:

[0007] S1, uniformly mixing a dispersion medium, a stabilizer, an initiator and a monomer to obtain a first mixture;

[0008] S2, subjecting the first mixture to step-by-step polymerization to obtain a second mixture;

[0009] S3, separating the second mixture to obtain acrylate polymer microspheres;

[0010] The dispersion medium and the monomer are immiscible with each other;

[0011] Wherein, the step-by-step polymerization is N-step polymerization, N≥2;

[0012] The monomer conversion rate in the Nth step is 1 to 5 times the monomer conversion rate in the N-1th step.

[0013] The second aspect of the present invention provides acrylic polymer microspheres prepared by the preparation method described in the first aspect of the present invention.

[0014] The third aspect of the present invention provides a use of the acrylic polymer microspheres described in the second aspect of the present invention as a modifier in a polyolefin film.

[0015] The fourth aspect of the present invention provides a system for preparing the acrylic polymer microspheres according to the second aspect of the present invention, characterized in that the system comprises: a raw material tank (1), a reactor (3), a collection tank (4), a separation device (5) and a heater (6);

[0016] The outlet of the raw material tank (1) is connected to the inlet of the reactor (3) for mixing the raw materials to obtain a first mixture;

[0017] The inlet of the reactor (3) is connected to the outlet of the raw material tank (1), and a heater (6) is provided outside the reactor (3) for polymerizing the first mixture to obtain a second mixture;

[0018] The inlet of the collecting tank (4) is connected to the outlet of the reactor (3) for collecting the second mixture;

[0019] The inlet of the separation device (5) is connected to the outlet of the collection tank (4) and is used to separate the collected second mixture to obtain acrylate polymer microspheres;

[0020] The number of the reactors 3 is M, the number of the heaters 6 is P, M≥2, P≥2.

[0021] Through the above technical scheme, the acrylate polymer microspheres and the preparation method and application thereof, and the system for preparing acrylate polymer microspheres provided by the present invention obtain the following beneficial effects: in the method, the polymerization reaction is carried out step by step, so that the heat transfer of the polymerization reaction system is easier to control, and it is further easier to remove the reaction heat in the reaction process, thereby improving the uniformity of the prepared polymer microspheres. At the same time, the dispersion medium and the monomer are mutually immiscible, and the polymer microspheres prepared by the above preparation method have the characteristics of suitable particle size, small dispersion coefficient, and narrow molecular weight distribution index. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a scanning electron microscope image of the acrylic polymer microspheres prepared in Example 1 of the present invention;

[0023] Figure 2 Schematic diagram of a system for preparing acrylic polymer microspheres according to Example 1 of the present invention.

[0024] Description of Reference Numerals

[0025] 1 raw material tank; 2-1 first chromatography pump; 2-2 second chromatography pump; 2-3 third chromatography pump; 3-1 first reactor; 3-2 second reactor; 3-3 third reactor; 4 collecting tank; 5 separation device; 6-1 first heater; 6-2 second heater; 6-3 third heater; 7 drying device; 8 condenser; 9 recovery tank. DETAILED DESCRIPTION

[0026] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0027] The first aspect of the present invention provides a method for preparing acrylic polymer microspheres, characterized in that the method comprises the following steps:

[0028] S1, uniformly mixing a dispersion medium, a stabilizer, an initiator and a monomer to obtain a first mixture;

[0029] S2, subjecting the first mixture to step-by-step polymerization to obtain a second mixture;

[0030] S3, separating the second mixture to obtain acrylate polymer microspheres;

[0031] The dispersion medium and the monomer are immiscible with each other;

[0032] Wherein, the step-by-step polymerization is N-step polymerization, N≥2;

[0033] The monomer conversion rate in the Nth step is 1 to 5 times the monomer conversion rate in the N-1th step.

[0034] In the present invention, the inventors have found that by carrying out the polymerization reaction in steps and controlling the monomer conversion rate in each step of the polymerization reaction to meet the above-mentioned range, the reaction for preparing acrylic polymer microspheres can be made easier to control, thereby facilitating the removal of reaction heat during the reaction and improving the uniformity of the polymer microspheres.

[0035] Furthermore, the dispersion medium and the monomer are immiscible with each other, and the prepared polymer microspheres have the characteristics of suitable particle size, small dispersion coefficient and narrow molecular weight distribution index.

[0036] In the present invention, the method further comprises, before the system is activated, first purging the system. The purging method is a conventional protective gas purging method in the art, such as nitrogen or inert gas purging. The purging time is not particularly limited, for example, it can be 20-40 minutes.

[0037] In the present invention, the monomer conversion rate in the Nth step is 1-2.5 times the monomer conversion rate in the N-1th step.

[0038] According to the present invention, in step S1, the mixing includes stirring and nitrogen bubbling.

[0039] In the present invention, the mixing is performed by combining stirring and bubbling, so that the stabilizer, the initiator and the monomer can be mixed more uniformly.

[0040] According to the present invention, the stirring rate of the stirring is 5-200 r / min, preferably 50-200 r / min; the stirring time is 5-40 min, preferably 10-40 min.

[0041] According to the present invention, the nitrogen bubbling time is 10-40 min, preferably 10-30 min.

[0042] According to the present invention, in step S2, the stepwise polymerization includes heating the first mixture through a plurality of temperature zones.

[0043] According to the present invention, the heating conditions of each of the multiple temperature zones independently include: a temperature of 45-95° C. and a time of 60-400 min.

[0044] In the present invention, the inventors have found that by controlling the temperature and time in each temperature zone to meet the above range, the monomer conversion rate in each step of the polymerization reaction can be controlled, thereby making it easier to control the reaction heat of the reaction system, and then prepare polymer microspheres with suitable particle size, small dispersion coefficient, and narrow molecular weight distribution index.

[0045] According to the present invention, the first mixture is heated through 3-5 temperature zones.

[0046] According to the present invention, the method further comprises: drying the acrylate polymer microspheres obtained after separation.

[0047] According to the present invention, the drying conditions include: a drying temperature of 50-120° C., a drying pressure of -0.95 to 0 MPaG, and a drying time of 300-720 min.

[0048] According to the present invention, the dispersion medium is selected from at least one of methanol, ethanol and propanol.

[0049] In the present invention, the dispersion medium is selected from the above types, and the prepared polymer microspheres have a smaller dispersion coefficient and a narrower molecular weight distribution index.

[0050] According to the present invention, the weight average molecular weight of the stabilizer is 10,000-600,000 g / mol.

[0051] In the present invention, the weight average molecular weight of the stabilizer satisfies the above range, which can ensure the formation of a stable polymer colloid dispersion system.

[0052] Furthermore, the weight average molecular weight of the stabilizer is 10,000-300,000 g / mol.

[0053] According to the present invention, the stabilizer is selected from polyvinyl pyrrolidone and / or polyacrylic acid.

[0054] According to the present invention, the initiator is selected from azo initiators and / or peroxide initiators.

[0055] According to the present invention, the initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dibenzoyl peroxide.

[0056] According to the present invention, the monomer is selected from methyl methacrylate and / or methyl acrylate.

[0057] According to the present invention, in the first mixture, the concentration of the monomer is 1-10 wt %.

[0058] According to the present invention, the content of the stabilizer is 3-10 wt % of the mass of the monomer.

[0059] According to the present invention, the content of the initiator is 0.2-2 wt % of the mass of the monomer.

[0060] In the present invention, when any one of the concentration of the monomer, the amount of the stabilizer and the amount of the initiator meets the above range, the polymerization reaction can be smoothly carried out, thereby improving the reaction efficiency of the polymerization reaction.

[0061] Furthermore, in the first mixture, the concentration of the monomer is 2-10 wt %.

[0062] Furthermore, the amount of the stabilizer is 4-10 wt % of the monomer mass.

[0063] Furthermore, the amount of the initiator used is 0.5-2 wt % of the mass of the monomer.

[0064] The second aspect of the present invention provides acrylic polymer microspheres prepared by the preparation method described in the first aspect of the present invention.

[0065] According to the present invention, the dispersion coefficient of the acrylic polymer microspheres is 1.008-1.1, preferably 1.008-1.09.

[0066] According to the present invention, the number average particle size of the acrylic polymer microspheres is 0.5-1.4 μm, preferably 0.8-1.4 μm.

[0067] According to the present invention, the weight average particle size of the acrylic polymer microspheres is 0.5-1.5 μm, preferably 0.8-1.5 μm.

[0068] According to the present invention, the number average molecular weight of the acrylic polymer microspheres is 15,000-50,000, preferably 20,000-40,000.

[0069] According to the present invention, the molecular weight distribution index of the acrylic ester polymer microspheres is 1.5-2.2, preferably 1.5-2.

[0070] The third aspect of the present invention provides a use of the acrylic polymer microspheres described in the second aspect of the present invention as a modifier in a polyolefin film.

[0071] In the present invention, the inventors found that higher haze can be obtained by applying acrylic polymer microspheres as a modifier to polyolefin films.

[0072] In the present invention, when the acrylate polymer microspheres are used as a modifier in a polyolefin film, the amount of the acrylate polymer microspheres is 5-35wt%, preferably 15-25wt%.

[0073] According to a preferred embodiment of the present invention, the polyolefin is polyethylene.

[0074] The fourth aspect of the present invention provides a system for preparing the acrylic polymer microspheres according to the second aspect of the present invention, characterized in that the system comprises: a raw material tank (1), a reactor (3), a collection tank (4), a separation device (5) and a heater (6);

[0075] The outlet of the raw material tank (1) is connected to the inlet of the reactor (3) for mixing the raw materials to obtain a first mixture;

[0076] The inlet of the reactor (3) is connected to the outlet of the raw material tank (1), and a heater (6) is provided outside the reactor (3) for polymerizing the first mixture to obtain a second mixture;

[0077] The inlet of the collecting tank (4) is connected to the outlet of the reactor (3) for collecting the second mixture;

[0078] The inlet of the separation device (5) is connected to the outlet of the collection tank (4) and is used to separate the collected second mixture to obtain acrylate polymer microspheres;

[0079] Wherein, the number of the reactors 3 is M, the number of the heaters 6 is P, M≥2, P≥2;

[0080] Along the flow direction of the reaction materials, the pipeline length of each reactor 3 decreases.

[0081] In the present invention, the separation device may be a separation device commonly used in the art, such as a centrifuge or a filtering device with a filtering material having a pore size of ≤3 microns.

[0082] According to an implementation method of the present invention, the rotation speed range of the centrifuge is 2000-10000r / min.

[0083] In the present invention, the heater can be a water bath device or an oil bath device, and the control accuracy is ±1°C.

[0084] In the present invention, the raw material tank (1) and the collection tank (4) contain stirring devices for mixing the materials evenly.

[0085] According to the present invention, the system further comprises: a pump (2), a drying device (7), a condenser (8) and a recovery tank (9);

[0086] The pump (2) is arranged before the reactor (3) and is used to pump the first mixture into the reactor (3);

[0087] The separation device (5) comprises a liquid phase outlet and a solid phase outlet;

[0088] The inlet of the drying device (7) is connected to the solid phase outlet of the separation device (5) and is used to dry the solid phase material obtained after separation of the second mixture;

[0089] The inlet of the condenser (8) is connected to the outlet of the drying device (7) and is used to condense the liquid phase in the drying device (7) to obtain a condensate;

[0090] The recovery tank (9) is connected to the outlet of the condenser (8) and is used to recover the condensate;

[0091] The recovery tank (9) is in communication with the liquid phase outlet of the separation device (5) and is used to recover the liquid phase material obtained after separation of the second mixture.

[0092] In the present invention, after the solid phase material is dried, the volatilized solvent is condensed by a condenser (8) and then enters a recovery tank (9), thereby preventing the solvent from leaking into the environment and causing pollution.

[0093] According to the present invention, the reactor 3 is a tubular microreactor.

[0094] According to the present invention, the inner diameter of the pipe of the reactor 3 is 0.1-5 mm; the length is 0.2-5 m.

[0095] In the present invention, the inner diameter and length of the pipe of the reactor 3 meet the above ranges, which can ensure the heat transfer of the reaction and enable the reaction to proceed smoothly.

[0096] Furthermore, the inner diameter of the pipe of the reactor 3 is 0.1-1 mm; and the length is 0.4-5 m.

[0097] According to a preferred embodiment of the present invention, the inner diameter of the pipeline of each reactor 3 increases gradually along the flow direction of the reaction materials.

[0098] According to the present invention, along the flow direction of the reaction materials, the inner diameter of the pipeline of the Mth reactor 3 is 1-2 times, preferably 1-1.5 times, the inner diameter of the pipeline of the M-1th reactor 3.

[0099] According to the present invention, along the flow direction of the reaction materials, the length of the pipeline of the Mth reactor 3 is 5-1 times, preferably 2.5-1 times, the length of the pipeline of the M-1th reactor 3.

[0100] In the present invention, the inner diameter and length of the pipeline of the reactor meet the above requirements, which can make the material react more completely, and further meet the preferred range, which can make the material react more thoroughly and make the reaction run smoothly, avoiding equipment shutdown or pipeline blockage.

[0101] In the present invention, the pump (2) may be a conventional pump in the art, for example, a chromatography pump.

[0102] According to the present invention, the rated output pressure of the pump (2) is 0.3-3 MPa, preferably 1-2.5 MPa.

[0103] According to the present invention, the flow rate of the reaction material in the system is 0.1-10 mL / min.

[0104] In the present invention, the flow rate of the reaction material in the system satisfies the above range, and the reaction can run smoothly.

[0105] Furthermore, the flow rate of the reaction material in the system is 0.1-8 mL / min.

[0106] Combination Figure 2 , the method and system of the present invention are further described:

[0107] The system is fully purged with nitrogen for 20-40 minutes. A dispersion medium, a stabilizer (weight average molecular weight of 10000-600000 g / mol), an initiator and a monomer are added to a raw material tank (1), and stirring is started at a speed of 5-200 r / min for 5-40 minutes. During the stirring process, nitrogen is introduced into the raw material tank (1) for bubbling for 10-40 minutes to fully dissolve the raw materials to obtain a first mixture. Wherein, based on the total mass of the first mixture, the mass concentration of the monomer is 1-10wt%, the content of the stabilizer is 3-10wt% of the mass of the monomer, and the content of the initiator is 0.2-2wt% of the mass of the monomer.

[0108] The first chromatographic pump (2-1), the second chromatographic pump (2-2) and the third chromatographic pump (2-3) are turned on in sequence. The first mixture is sent into the first reactor (3-1) through the first chromatographic pump (2-1). The first reactor (3-1) is provided with a first heater (6-1) outside with a control accuracy of ±1°C for heating the first mixture and performing a first polymerization reaction in the first reactor (3-1) to obtain a second mixture I; the rated output pressure of the first chromatographic pump (2-1) is 0.3-3MPa, the inner diameter of the pipeline of the first reactor (3-1) is 0.1-5mm, and the length is 0.2-5m. The first polymerization reaction conditions include: temperature of 45-95°C, time of 60-400min, and material flow rate of 0.1-10mL / min;

[0109] The second mixture I is sent into the second reactor (3-2) through the second chromatographic pump (2-2); the second reactor (3-2) is provided with a second heater (6-2) outside with a control accuracy of ±1°C for heating the second mixture I, and a second polymerization reaction is carried out in the second reactor (3-2) to obtain a second mixture II; the rated output pressure of the second chromatographic pump (2-2) is 0.3-3MPa, the inner diameter of the pipeline of the second reactor (3-2) is 0.1-5mm, and the length is 0.2-5m; the second polymerization reaction conditions include: temperature of 45-95°C, time of 60-400min, and material flow rate of 0.1-10mL / min;

[0110] The second mixture II is sent into the third reactor (3-3) through the third chromatographic pump (2-3); the third reactor (3-3) is provided with a third heater (6-3) outside with a control accuracy of ±1°C for heating the second mixture II, and a third polymerization reaction is carried out in the third reactor (3-3) to obtain a second mixture III; the rated output pressure of the third chromatographic pump (2-3) is 0.3-3MPa, the inner diameter of the pipeline of the third reactor (3-3) is 0.1-5mm, and the length is 0.2-5m; the third polymerization reaction conditions include: temperature of 45-95°C, time of 60-400min, and material flow rate of 0.1-10mL / min;

[0111] The inlet of the collecting tank (4) is connected to the outlet of the third reactor (3-3), and is used to collect the second mixture III and mix it uniformly at a stirring rate of 5-200 r / min;

[0112] The inlet of the separation device (5) is connected to the outlet of the collection tank (4), and is used to separate the collected second mixture III to obtain a solid phase material and a liquid phase material;

[0113] The separation device (5) comprises a liquid phase outlet and a solid phase outlet, and the inlet of the drying device (7) is connected to the solid phase outlet of the separation device (5), and is used to dry the solid phase material obtained after separation of the second mixture to obtain acrylic polymer microspheres and a volatilized liquid phase; wherein the drying conditions include: a drying temperature of 50-120° C., a drying pressure of -0.95 to 0 MPaG, and a drying time of 300-720 min;

[0114] The inlet of the condenser (8) is connected to the outlet of the drying device (7) and is used to condense the liquid phase volatilized in the drying device (7) to obtain a condensate;

[0115] The recovery tank (9) is connected to the outlet of the condenser (8) and is used to recover the condensate;

[0116] The recovery tank (9) is connected to the liquid phase outlet of the separation device (5) and is used to recover the liquid phase material obtained after the second mixture III is separated.

[0117] The present invention will be described in detail below by way of examples. In the following examples,

[0118] The morphology of the polymers was observed using a Hitachi S-4800 scanning electron microscope.

[0119] The particle size of the polymer was measured by scanning electron microscopy graphics software;

[0120] The number average molecular weight of the polymers was measured by gel permeation chromatography;

[0121] The weight average molecular weight of the stabilizer was measured by gel permeation chromatography;

[0122] The molecular weight distribution index of the polymer was measured by gel permeation chromatography;

[0123] The monomer conversion rate was calculated by the following formula:

[0124]

[0125] Where m1 is the mass of the obtained polymer and m0 is the mass of the added monomer.

[0126] The number average particle size is Where n is the number of particles, di is the particle size of the i-th particle;

[0127] The weight average particle size is Where n is the number of particles, di is the particle size of the i-th particle;

[0128] The dispersion coefficient is P = Dw / Dn.

[0129] The raw materials involved in the examples and comparative examples are all conventional commercial products in the art.

[0130] Example 1

[0131] The system is fully purged with nitrogen for 20 minutes. 888.5g of ethanol as a dispersion medium, 10g of polyvinyl pyrrolidone as a stabilizer (weight average molecular weight of 100,000 g / mol), 1.5g of azobisisobutyronitrile as an initiator and 100g of methyl methacrylate as a monomer are added to a raw material tank (1), stirring is started at a speed of 150 r / min for 20 minutes. During the stirring process, nitrogen is introduced into the raw material tank (1) for bubbling for 30 minutes to fully dissolve the raw materials to obtain a first mixture. Wherein, based on the total mass of the first mixture, the mass concentration of methyl methacrylate is 10wt%, the content of polyvinyl pyrrolidone is 10wt% of the mass of methyl methacrylate, and the content of azobisisobutyronitrile is 1.5wt% of the mass of methyl methacrylate.

[0132] The first chromatographic pump (2-1), the second chromatographic pump (2-2) and the third chromatographic pump (2-3) are turned on in sequence. The first mixture is sent into the first reactor (3-1) through the first chromatographic pump (2-1). The first reactor (3-1) is provided with a first heater (6-1) (water bath) with an accuracy of ±1°C for heating the first mixture, and a first polymerization reaction is carried out in the first reactor (3-1) to obtain a second mixture I, at which the conversion rate of methyl methacrylate is 36.7%; the rated output pressure of the first chromatographic pump (2-1) is 2.5MPa, the inner diameter of the pipeline of the first reactor (3-1) is 0.1mm, and the length is 5m. The first polymerization reaction conditions include: temperature of 75°C, time of 392.5min, and material flow rate of 0.1mL / min;

[0133] The second mixture I is fed into the second reactor (3-2) through the second chromatographic pump (2-2), and the second reactor (3-2) is provided with a second heater (6-2) (water bath) outside with a control accuracy of ±1°C for heating the second mixture I, and a second polymerization reaction is carried out in the second reactor (3-2) to obtain a second mixture II, wherein the conversion rate of methyl methacrylate is 66%; the rated output pressure of the second chromatographic pump (2-2) is 2.5 MPa, the inner diameter of the pipeline of the second reactor (3-2) is 0.1 mm, and the length is 4 m, and the second polymerization reaction conditions include: temperature of 75°C, time of 314 min, and material flow rate of 0.1 mL / min;

[0134] The second mixture II is sent into the third reactor (3-3) through the third chromatographic pump (2-3), and the third reactor (3-3) is provided with a third heater (6-3) (water bath) outside, with a control accuracy of ±1°C, for heating the second mixture II, and performing a third polymerization reaction in the third reactor (3-3) to obtain a second mixture III, wherein the conversion rate of methyl methacrylate is 88%; the rated output pressure of the third chromatographic pump (2-3) is 2.5 MPa, the inner diameter of the pipeline of the third reactor (3-3) is 0.1 mm, and the length is 3 m, and the third polymerization reaction conditions include: temperature of 80°C, time of 235.5 min, and material flow rate of 0.1 mL / min;

[0135] The inlet of the collecting tank (4) is connected to the outlet of the third reactor (3-3), and is used to collect the second mixture III and mix it uniformly at a speed of 150 r / min;

[0136] The inlet of the separation device (5) (centrifuge) is connected to the outlet of the collection tank (4), and is used to separate the collected second mixture III to obtain solid phase material and liquid phase material, wherein the rotation speed range of the centrifuge is 6000r / min;

[0137] The separation device (5) comprises a liquid phase outlet and a solid phase outlet, and the inlet of the drying device (7) is connected to the solid phase outlet of the separation device (5), and is used to dry the solid phase material obtained after separation of the second mixture to obtain acrylate polymer microspheres A1 and a volatilized liquid phase; wherein the drying conditions include: a drying temperature of 80° C., a drying pressure of -0.8 MPaG, and a drying time of 720 min;

[0138] The inlet of the condenser (8) is connected to the outlet of the drying device (7) and is used to condense the liquid phase volatilized in the drying device (7) to obtain a condensate;

[0139] The recovery tank (9) is connected to the outlet of the condenser (8) and is used to recover the condensate;

[0140] The recovery tank (9) is connected to the liquid phase outlet of the separation device (5) and is used to recover the liquid phase material obtained after the second mixture III is separated.

[0141] The morphology of polymer microsphere A1 product is as follows Figure 1 As shown. Figure 1 It can be seen that the obtained polymer microspheres A1 are monodisperse microspheres with smooth surfaces. The number average molecular weight of polymer microspheres A1 is 40,000 g / mol, the molecular weight distribution is 1.62, the weight average particle size is 1.265 μm, the number average particle size is 1.25 μm, and the dispersion coefficient is 1.012.

[0142] Example 2

[0143] The method of Example 1 is used, except that, based on the total mass of the first mixture, the mass concentration of methyl methacrylate is 10wt%, the amount of polyvinyl pyrrolidone is 8wt% of the mass of methyl methacrylate used, and the amount of azobisisobutyronitrile is 2wt% of the mass of methyl methacrylate;

[0144] The inner diameter of the pipe of the first reactor (3-1) is 0.5 mm, the length is 5 m, the material flow rate is 5 mL / min, and the methyl methacrylate conversion rate is 36.3%;

[0145] The inner diameter of the pipeline of the second reactor (3-2) is 0.5 mm, the length is 4 m, the material flow rate is 5 mL / min, and the methyl methacrylate conversion rate is 65.3%;

[0146] The inner diameter of the pipeline of the third reactor (3-3) is 0.5 mm, the length is 3 m, the material flow rate is 5 mL / min, and the methyl methacrylate conversion rate is 87%;

[0147] The speed range of the centrifuge is 5000r / min.

[0148] Finally, polymer microspheres A2 were obtained, and the number average molecular weight of polymer microspheres A2 was 37,000 g / mol, the molecular weight distribution was 1.73, the weight average particle size was 1.102 μm, the number average particle size was 1.014 μm, and the dispersion coefficient was 1.087.

[0149] Example 3

[0150] The method of Example 2 was followed, except that the inner diameter of the pipe of the first reactor (3-1) was 1 mm, and the conversion rate of methyl methacrylate was 65.7%;

[0151] The inner diameter of the pipe of the second reactor (3-2) is 1 mm, the length is 1 m, and the conversion rate of methyl methacrylate is 78.9%;

[0152] The inner diameter of the pipe of the third reactor (3-3) is 1 mm, the length is 1 m, and the conversion rate of methyl methacrylate is 92%.

[0153] Finally, polymer microspheres A3 were obtained, and the number average molecular weight of polymer microspheres A3 was 35,000 g / mol, the molecular weight distribution was 1.76, the weight average particle size was 1.002 μm, the number average particle size was 0.98 μm, and the dispersion coefficient was 1.022.

[0154] Example 4

[0155] The method of Example 1 is used, except that, based on the total mass of the first mixture, the mass concentration of methyl methacrylate is 5wt%, the amount of polyvinyl pyrrolidone (weight average molecular weight of 50000 g / mol) is 6wt% of the mass of methyl methacrylate used, and the initiator is azobisisoheptanenitrile, and the amount used is 2wt% of the mass of methyl methacrylate;

[0156] The inner diameter of the pipe of the first reactor (3-1) is 0.5 mm and the length is 5 m;

[0157] The first polymerization reaction conditions include: temperature of 50° C., material flow rate of 5 mL / min, and methyl methacrylate conversion rate of 71.3%;

[0158] The second polymerization reaction conditions include: temperature of 55° C., material flow rate of 5 mL / min, and methyl methacrylate conversion rate of 85.6%;

[0159] The third polymerization reaction conditions include: temperature of 60° C., material flow rate of 5 mL / min, and methyl methacrylate conversion rate of 86%;

[0160] The rotation speed of the centrifuge is 8000r / min.

[0161] Finally, polymer microspheres A4 were obtained, and the number average molecular weight of polymer microspheres A4 was 34,000 g / mol, the molecular weight distribution was 1.78, the weight average particle size was 0.956 μm, the number average particle size was 0.933 μm, and the dispersion coefficient was 1.025.

[0162] Example 5

[0163] The method of Example 1 is followed, except that the dispersion medium is replaced by propanol, the weight average molecular weight of polyvinyl pyrrolidone is 10000 g / mol, and the initiator is replaced by dibenzoyl peroxide.

[0164] Based on the total mass of the first mixture, the mass concentration of methyl methacrylate is 8wt%, the amount of polyvinyl pyrrolidone is 8wt% of the mass of methyl methacrylate used, and the amount of initiator is 2wt% of the mass of methyl methacrylate.

[0165] The inner diameter of the pipe of the first reactor (3-1) is 4 mm, the length is 0.4 m, the material flow rate is 10 mL / min, and the methyl methacrylate conversion rate is 38.7%;

[0166] The inner diameter of the pipeline of the second reactor (3-2) is 4 mm, the length is 0.3 m, the material flow rate is 10 mL / min, and the methyl methacrylate conversion rate is 67.7%;

[0167] The inner diameter of the pipeline of the third reactor (3-3) is 4 mm, the length is 0.2 m, the material flow rate is 10 mL / min, and the conversion rate of methyl methacrylate is 87%.

[0168] The first polymerization reaction conditions include: a temperature of 80°C;

[0169] The second polymerization reaction conditions include: a temperature of 85°C;

[0170] The third polymerization reaction conditions include: a temperature of 90°C.

[0171] Finally, polymer microspheres A5 were obtained, and the number average molecular weight of polymer microspheres A5 was 32,000 g / mol, the molecular weight distribution was 1.88, the weight average particle size was 0.938 μm, the number average particle size was 0.905 μm, and the dispersion coefficient was 1.036.

[0172] Example 6

[0173] The method of Example 1 was followed, except that the flow rate was 10.5 mL / min;

[0174] The conversion rate of methyl methacrylate in the first reactor (3-1) is 3.67%;

[0175] The conversion rate of methyl methacrylate in the second reactor (3-2) is 6.6%;

[0176] The methyl methacrylate conversion rate of the third reactor (3-3) is 8.5%;

[0177] The speed range of the centrifuge is 5000r / min.

[0178] Finally, polymer microspheres A6 were obtained, and the number average molecular weight of polymer microspheres A6 was 45000 g / mol, the molecular weight distribution was 1.61, the weight average particle size was 0.512 μm, the number average particle size was 0.507 μm, and the dispersion coefficient was 1.01.

[0179] Example 7

[0180] The method of Example 1 was followed, except that bubbling was not performed.

[0181] Finally, polymer microspheres A7 were obtained, and the number average molecular weight of polymer microspheres A7 was 42000 g / mol, the molecular weight distribution was 1.63, the weight average particle size was 1.21 μm, the number average particle size was 1.194 μm, and the dispersion coefficient was 1.013.

[0182] Example 8

[0183] The method of Example 1 is different from that of Example 1:

[0184] The material flow rate of the first reactor (3-1) is 0.5 mL / min, and the conversion rate of methyl methacrylate is 7.17%;

[0185] The material flow rate of the second reactor (3-2) is 0.2 mL / min, and the conversion rate of methyl methacrylate is 21.5%;

[0186] The material flow rate of the third reactor (3-3) is 0.1 mL / min, and the conversion rate of methyl methacrylate is 43%;

[0187] Finally, polymer microspheres A8 were obtained, and the number average molecular weight of polymer microspheres A8 was 38000 g / mol, the molecular weight distribution was 1.64, the weight average particle size was 0.871 μm, the number average particle size was 0.835 μm, and the dispersion coefficient was 1.043.

[0188] Comparative Example 1

[0189] Add the same raw materials as in Example 1 to the autoclave, start stirring, and stir at a speed of 200 r / min to allow the added raw materials to be fully mixed and dissolved. During the stirring process, nitrogen is introduced into the autoclave to bubble the liquid system for 30 minutes. React at 75°C for 10 hours. Separate and obtain polymer D1, at which point the conversion rate of methyl methacrylate is 85%. The number average molecular weight of polymer D1 is 25000 g / mol, the molecular weight distribution is 2.8, the weight average particle size is 1.41 μm, the number average particle size is 1.12 μm, and the dispersion coefficient is 1.259.

[0190] Comparative Example 2

[0191] The method of Example 1 was followed, except that the dispersion medium was replaced with an equal amount of ethyl acetate. The pipeline was clogged and a spherical polymer dispersion could not be obtained.

[0192] Comparative Example 3

[0193] The method of Example 1 is as follows, except that the inner diameter of the pipe of the first reactor (3-1) is 0.1 mm, the length is 0.5 m, the material flow rate is 2 mL / min, and the methyl methacrylate conversion rate is 0.26%;

[0194] The inner diameter of the pipeline of the second reactor (3-2) is 0.1 mm, the length is 1 m, the material flow rate is 0.5 mL / min, and the methyl methacrylate conversion rate is 2.09%;

[0195] The inner diameter of the pipeline of the third reactor (3-3) is 0.1 mm, the length is 8 m, the material flow rate is 0.1 mL / min, and the third pump stops working due to overpressure, and the reaction process cannot proceed smoothly.

[0196] Comparative Example 4

[0197] The method of Example 1 was followed, except that there was only one chromatographic pump, one reactor with a diameter of 0.1 mm and a length of 5 m, and one heater, and the reactor was directly connected to the collection tank. The conversion rate of methyl methacrylate was 35%, and polymer microspheres D4 were obtained, with a number average molecular weight of 45,000 g / mol and a molecular weight distribution of 1.59. The weight average particle size was 0.48 μm, the number average particle size was 0.475 μm, and the dispersion coefficient was 1.011.

[0198] Table 1

[0199]

[0200]

[0201] In order to further illustrate that the polymer microspheres prepared by the present invention can be well applied to polyethylene films, the polymer microspheres prepared in the examples and comparative examples were added to polyethylene films without adding any other additives. The haze effect of the obtained film was tested according to GB / T2410-2008, and the results are shown in Table 2.

[0202] Table 2

[0203]

[0204]

[0205] *No additives added

[0206] From the contents of Table 2, it can be seen that when the polymer microspheres prepared in Examples 1-8 of the present invention are applied to polyethylene, the haze of the polyethylene film can reach at least 87%.

[0207] Further satisfying the preferred embodiments 1-4 of the present invention, the haze of the polyethylene film can be no less than 94%.

[0208] Among them, without adding any external additives, the polyethylene film with calcium carbonate or silicon dioxide added has obvious crystal points (fish eyes) visible to the naked eye, while the polyethylene film with the microspheres of the present invention added has no fish eyes.

[0209] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing acrylic polymer microspheres, characterized in that: The method comprises the following steps: S1, uniformly mixing a dispersion medium, a stabilizer, an initiator and a monomer to obtain a first mixture; S2, subjecting the first mixture to step-by-step polymerization to obtain a second mixture; S3, separating the second mixture to obtain acrylate polymer microspheres; The dispersion medium and the monomer are immiscible with each other; Wherein, the step-by-step polymerization is N-step polymerization, N≥2; The monomer conversion rate in the Nth step is 1 to 5 times the monomer conversion rate in the N-1th step.

2. The preparation method according to claim 1, wherein The monomer conversion rate of the Nth step is 1-2.5 times the monomer conversion rate of the N-1th step; Preferably, in step S1, the mixing includes stirring and nitrogen bubbling; Preferably, the stirring rate of the stirring is 5-200 r / min, preferably 50-200 r / min; the stirring time is 5-40 min, preferably 10-40 min; Preferably, the nitrogen bubbling time is 10-40 min, preferably 10-30 min.

3. The preparation method according to claim 1 or 2, wherein In step S2, the stepwise polymerization includes heating the first mixture through a plurality of temperature zones; Preferably, the heating conditions of each of the multiple temperature zones independently include: temperature of 45-95°C, time of 60-400 min; Preferably, the first mixture is heated through 3-5 temperature zones.

4. The method according to any one of claims 1 to 3, wherein: The method further comprises: drying the acrylate polymer microspheres obtained after separation; Preferably, the drying conditions include: drying temperature of 50-120° C., drying pressure of -0.95 to 0 MPaG, and drying time of 300-720 min.

5. The preparation method according to any one of claims 1 to 4, wherein: The dispersion medium is selected from at least one of methanol, ethanol and propanol; Preferably, the weight average molecular weight of the stabilizer is 10,000-600,000 g / mol, preferably 10,000-300,000 g / mol; Preferably, the stabilizer is selected from polyvinyl pyrrolidone and / or polyacrylic acid; Preferably, the initiator is selected from azo initiators and / or peroxide initiators; Preferably, the initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dibenzoyl peroxide; Preferably, the monomer is selected from methyl methacrylate and / or methyl acrylate.

6. The preparation method according to any one of claims 1 to 5, wherein: In the first mixture, the concentration of the monomer is 1-10wt%, preferably 2-10wt%; Preferably, the amount of the stabilizer is 3-10wt% of the mass of the monomer, preferably 4-10wt%; Preferably, the amount of the initiator used is 0.2-2 wt %, preferably 0.5-2 wt %, based on the weight of the monomer.

7. Acrylate polymer microspheres prepared by the preparation method according to any one of claims 1 to 6.

8. The polymer microspheres according to claim 7, wherein The dispersion coefficient of the acrylic polymer microspheres is 1.008-1.1, preferably 1.008-1.09; Preferably, the number average particle size of the acrylic polymer microspheres is 0.5-1.4 μm, preferably 0.8-1.4 μm; Preferably, the weight average particle size of the acrylic polymer microspheres is 0.5-1.5 μm, preferably 0.8-1.5 μm; Preferably, the number average molecular weight of the acrylate polymer microspheres is 15,000-50,000 g / mol, preferably 20,000-40,000 g / mol; Preferably, the molecular weight distribution index of the acrylic polymer microspheres is 1.5-2.2, preferably 1.5-2.

9. Use of the acrylic polymer microspheres according to claim 7 or 8 as a modifier in polyolefin films.

10. A system for preparing the acrylic polymer microspheres according to claim 7 or 8, characterized in that: The system comprises: a raw material tank 1, a reactor 3, a collecting tank 4, a separation device 5 and a heater 6; The outlet of the raw material tank 1 is connected to the inlet of the reactor 3, and is used to mix the raw materials to obtain a first mixture; The inlet of the reactor 3 is connected to the outlet of the raw material tank 1, and a heater 6 is provided outside the reactor 3 for polymerizing the first mixture to obtain a second mixture; The inlet of the collecting tank 4 is connected to the outlet of the reactor 3, and is used to collect the second mixture; The inlet of the separation device 5 is connected to the outlet of the collection tank 4, and is used to separate the collected second mixture to obtain acrylate polymer microspheres; Wherein, the number of the reactors 3 is M, the number of the heaters 6 is P, M≥2, P≥2; Along the flow direction of the reaction materials, the pipeline length of each reactor 3 decreases.

11. The system according to claim 10, wherein: The system further comprises: a pump 2, a drying device 7, a condenser 8 and a recovery tank 9; The pump 2 is disposed before the reactor 3 and is used to pump the first mixture into the reactor 3; The separation device 5 comprises a liquid phase outlet and a solid phase outlet; The inlet of the drying device 7 is connected to the solid phase outlet of the separation device 5, and is used to dry the solid phase material obtained after the second mixture is separated; The inlet of the condenser 8 is connected to the outlet of the drying device 7, and is used to condense the liquid phase in the drying device 7 to obtain a condensate; The recovery tank 9 is connected to the outlet of the condenser 8 and is used to recover the condensate; The recovery tank 9 is communicated with the liquid phase outlet of the separation device 5 and is used for recovering the liquid phase material obtained after the second mixture is separated.

12. The system according to claim 10 or 11, wherein: The reactor 3 is a tubular microreactor; Preferably, the inner diameter of the pipe of the reactor 3 is 0.1-5 mm, preferably 0.1-1 mm; the length is 0.2-5 m, preferably 0.4-5 m; Preferably, along the flow direction of the reaction materials, the inner diameter of the pipeline of each reactor 3 increases; Preferably, along the flow direction of the reaction materials, the inner diameter of the pipeline of the Mth reactor 3 is 1-2 times, preferably 1-1.5 times, the inner diameter of the pipeline of the M-1th reactor 3; Preferably, along the flow direction of the reaction materials, the length of the pipeline of the M-1th reactor 3 is 1-2 times, preferably 1-1.5 times, the length of the pipeline of the Mth reactor 3; Preferably, the rated output pressure of the pump 2 is 0.3-3 MPa, preferably 1-2.5 MPa; Preferably, the flow rate of the reaction material in the system is 0.1-10 mL / min, preferably 0.1-8 mL / min.

Citation Information

Patent Citations

  • Method of synthesizing monodisperse micron-level poly(methyl methacrylate) micro-sphere

    CN101054427A

  • Method and device for polymerizing polyacrylonitrile spinning stock solution

    CN101928368A

  • Crosslinked monodispersed polymer functional microspheres and preparation method thereof

    CN105001367A

  • Preparation method and preparation device for polyacrylamide nanoparticles

    CN110054727A

  • Production of microspherical copolymer having narrow particle diameter distribution