Rubber sole for outdoor sports and preparation method thereof

A rubber sole formulation with ethylene-vinyl acetate copolymer, polyvinyl alcohol, and anti-wear agents like corundum and wollastonite enhances cell structure strength and durability, addressing the weakness of chemically foamed soles.

CN119060461AInactive Publication Date: 2024-12-03DONGGUAN HENGRUILONG NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411319084.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Chemically foamed rubber soles have weak connections between pores, leading to fragile cell walls, reduced shock absorption, and decreased durability due to easy rupture or deformation, which is exacerbated in outdoor environments.

Method used

A rubber sole formulation comprising rubber, ethylene-vinyl acetate copolymer, polyvinyl alcohol, crosslinking agent, accelerator, vulcanizing agent, and foaming agent, with an anti-wear agent made of corundum, wollastonite, and cellulose fiber, optimized for uniform cell structure and enhanced cell wall strength.

Benefits of technology

The sole achieves improved air permeability, wear resistance, elasticity, and durability, maintaining structural integrity and shock absorption under external impacts and long-term wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005053187190000061
    Figure BDA0005053187190000061
  • Figure BDA0005053187190000071
    Figure BDA0005053187190000071
  • Figure BDA0005053187190000091
    Figure BDA0005053187190000091
Patent Text Reader

Abstract

The invention relates to the technical field of sole processing, in particular to a rubber sole for outdoor sports and a preparation method thereof.The rubber sole is prepared from, by weight, 40%-50% of rubber, 10%-15% of ethylene-vinyl acetate copolymer, 20%-30% of polyvinyl alcohol, 1%-2% of cross-linking agent, 0.3%-0.8% of accelerant, 0.5%-1% of vulcanizing agent, 3%-5% of foaming agent and the balance wear-resisting agent; the wear-resistant agent is obtained by mixing corundum, wollastonite and cellulosic fibers, and the rubber sole for outdoor sports, which is obtained according to the formula, has good air permeability, wear resistance, elasticity and durability, is light in weight and is not easy to damage in a use process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of sole processing, and more specifically, to a rubber sole for outdoor sports and a preparation method thereof. Background Art

[0002] Rubber soles have good wear resistance, anti-slip, oil resistance, acid and alkali resistance and water resistance, and at the same time have good softness and extensibility, and are not easy to get water in. For outdoor environments where you need to walk on slippery, rocky or uneven roads, rubber soles are an ideal choice.

[0003] However, the weight of the rubber sole may increase the burden on the foot when worn for a long time. At the same time, the air permeability of the rubber sole is relatively poor, which can easily cause stuffiness and discomfort in the feet, especially in high temperature or humid environments. In order to reduce the weight of the rubber sole and increase its air permeability, people have explored foam rubber soles. Foam rubber soles are a type of sole made of rubber material through a foaming process. A large number of tiny bubbles are formed inside the rubber, thereby reducing the density of the sole, making it light and breathable. Foam rubber mainly adopts two methods: physical foaming and chemical foaming. Among them, physical foaming is to accurately control the size and distribution of the bubbles by controlling parameters such as gas pressure and temperature, so as to obtain an ideal foaming effect. However, the physical foaming equipment is complex and the process requirements are high, so the production cost is relatively high, and the production efficiency is low, which is difficult to meet the needs of large-scale production, such as using supercritical carbon dioxide foaming.

[0004] The main foaming agent of chemical foaming decomposes at high temperature to produce gas, which expands the rubber material to form pores. The chemical foaming process is simple, the production cost is low, the production efficiency is high, and it is suitable for large-scale production. Therefore, most companies now use chemical foaming. However, in actual use, it is found that the connection between the pores of chemical foaming is not strong enough, resulting in relatively thin and fragile pore walls. When subjected to external impact or long-term wear, the pores are prone to rupture or deformation, resulting in weakened shock absorption performance, reduced elasticity, insufficient support, etc., which affects the durability and service life of the sole. Summary of the invention

[0005] In order to solve the problem that the connection between chemically foamed cells is not strong enough, resulting in relatively thin and fragile cell walls, the present application provides a rubber sole for outdoor sports and a preparation method thereof.

[0006] In a first aspect, the present application provides a rubber sole for outdoor sports, which adopts the following technical solution: a rubber sole for outdoor sports, prepared from the following raw materials in the following weight percentages: Rubber 40-50% Ethylene-vinyl acetate copolymer 10-15% Polyvinyl alcohol 20-30% Crosslinking agent 1-2% Accelerator 0.3-0.8% Vulcanizing agent 0.5-1% Foaming agent 3-5% The rest is anti-wear agent The wear-resistant agent is obtained by mixing corundum, wollastonite and cellulose fiber.

[0007] By adopting the above technical solution, the rubber sole for outdoor sports has good air permeability, wear resistance, elasticity and durability, is light in weight and is not easily damaged during use.

[0008] In the present application, the combination of rubber, ethylene-vinyl acetate copolymer and polyvinyl alcohol helps to form a more uniform and strong cell structure, wherein the flexibility of ethylene-vinyl acetate copolymer and the adhesiveness of polyvinyl alcohol work together to make the connection between cells more solid, the cell wall thickened, the cells not easy to break, and good stability, so that the sole can maintain structural integrity and enhance its durability when subjected to external impact or long-term wear. At the same time, the stability of the cell structure is improved, so that the sole has a stronger support force while providing a good shock-absorbing effect, which helps to maintain the shape stability of the sole and prevent deformation under long-term use or complex terrain.

[0009] In this application, the anti-wear agent is obtained by mixing corundum, wollastonite and cellulose fiber, and through the joint action of the three, the wear resistance of rubber soles is improved, and the structural strength of the pore wall can also be enhanced, so as to prevent the pores from breaking or deforming, and the service life of the sole is extended, and it is suitable for outdoor sports and other scenes that need to frequently contact the ground and bear large friction. Wherein, corundum has high hardness and good wear resistance, and is evenly distributed in the rubber matrix as a hard point, and can disperse and resist abrasive force, extend the service life of the sole, and can also increase the roughness of the sole, increase the friction between the sole and the ground, and enhance the grip of the sole. Wollastonite is a needle-shaped or fibrous silicate mineral, and its needle-shaped or fibrous structure enables wollastonite to form an effective reinforcing network in the rubber matrix, and in the foaming process, wollastonite particles can be embedded in the pore wall, increase the thickness and strength of the pore wall, and prevent the pore from breaking or deforming when subjected to external impact. Cellulose fiber can form a continuous mesh structure, which helps to firmly fix the corundum and wollastonite particles in the rubber matrix and is closely combined with the rubber matrix. The mesh structure can not only improve the strength and toughness of the sole, but also increase the wear resistance of the sole. At the same time, the cellulose fiber can also synergize with the wollastonite fiber and the corundum particles to further enhance the wear resistance and cell strength of the sole. Preferably, the cellulose fiber is one of hemp fiber, viscose fiber or microcrystalline cellulose.

[0010] The cross-linking agent promotes the cross-linking reaction between rubber molecules to form a three-dimensional network structure; the accelerator accelerates the vulcanization reaction rate; the vulcanizer cross-links and solidifies the rubber molecular chains to improve the strength and stability of rubber products. The above additives work together to enable the rubber sole to maintain excellent physical properties and chemical stability after foaming. By precisely controlling the amount of foaming agent and the vulcanization process, the size, distribution and density of the pores can be adjusted, thereby optimizing the pore structure.

[0011] Preferably, the weight ratio of the corundum, the wollastonite and the cellulose fiber is (2-5):(3-6):1.

[0012] By adopting the above technical solution, the usage ratio of corundum, wollastonite and cellulose fiber is optimized, and the wear resistance and pore structure stability of the rubber sole are further improved. At the same time, it also has good strength and toughness, which can meet the high requirements of outdoor sports for the sole. As a material with high hardness and high wear resistance, the content of corundum should not be too high so as not to reduce the flexibility of the rubber sole. The appropriate amount of wollastonite further enhances the wear resistance of the sole. Its fibrous structure helps to disperse the wear force, and at the same time complements the corundum particles to improve the wear resistance of the sole. The appropriate amount of cellulose fiber helps to firmly fix the corundum and wollastonite particles in the rubber matrix to form a stable reinforcement network, which not only improves the strength of the sole, but also maintains the good toughness of the sole.

[0013] Preferably, the average particle size of the corundum is 20-200 nm, the average particle size of the wollastonite is 100-300 nm, and the average particle size of the cellulose fiber is 150-250 nm.

[0014] By adopting the above technical solution, the average particle size of corundum, wollastonite and cellulose fiber is optimized, so that the three can be more closely combined with rubber, further improving the wear resistance and cell structure stability of the sole, so that the rubber sole can remain stable during long-term use. In addition, in harsh outdoor environments, the sole can effectively resist wear and damage, extending its service life.

[0015] Preferably, the rubber is obtained by mixing EPDM rubber and butadiene rubber in a weight ratio of 8:(3-5).

[0016] By adopting the above technical solution, the wear resistance and strength of the rubber sole are further improved. EPDM rubber itself has good wear resistance. After mixing with butyl rubber, the wear resistance of rubber products can be further improved, making it more suitable for occasions requiring high wear resistance. Butadiene rubber has high mechanical strength. After mixing with EPDM rubber, it can improve the mechanical strength of rubber products while maintaining a certain elasticity. The combination of the two can further improve the wear resistance, weather resistance, elasticity and comfort of rubber shoes used for outdoor sports.

[0017] Preferably, the foaming agent is obtained by mixing p-toluenesulfonyl hydrazide and diisopropyl azodicarboxylate in a weight ratio of (1-2):0.8.

[0018] By adopting the above technical solution, optimizing the type and amount of foaming agent, and controlling the rate and degree of foaming, it helps to ensure that the rubber sole forms an ideal microporous structure during the vulcanization process, thereby improving its elasticity and lightweight performance. At the same time, it helps to improve the air permeability and drainage of the sole, keeping the feet dry and comfortable.

[0019] Preferably, the crosslinking agent is one of dicumyl peroxide, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane or benzoyl peroxide.

[0020] By adopting the above technical solution, the type of cross-linking agent is optimized, the speed of the vulcanization reaction is controlled, and the chemical bond connection between the rubber molecular chains is promoted, so that the rubber sole has higher wear resistance, strength and elasticity. Preferably, the vulcanizing agent is one of sulfur or triallyl isocyanurate.

[0021] By adopting the above technical solution, the type of vulcanizing agent is optimized, and the cross-linking reaction between rubber molecular chains is promoted, so that stable chemical bonds are formed between the rubber molecular chains, thereby giving the rubber sole higher strength, wear resistance, durability and elasticity.

[0022] Preferably, the number average molecular weight of the polyvinyl alcohol is 25,000-120,000.

[0023] By adopting the above technical solution, within the range of number average molecular weight, polyvinyl alcohol can be better dispersed in rubber and form a stronger interaction with the rubber molecular chain, thereby enhancing the cohesive force of the rubber, reducing the merging and rupture of the cells during the formation process, and making the cell structure more uniform and dense. At the same time, it can also enhance the toughness of the cell wall to prevent the cells from easily rupturing when subjected to external impact.

[0024] Preferably, the ethylene content in the ethylene-vinyl acetate copolymer is 20-40 wt%.

[0025] By adopting the above technical solution, the ethylene content in ethylene-vinyl acetate copolymer is optimized, so that ethylene-vinyl acetate copolymer has good flexibility while maintaining a certain rigidity, which helps to adjust the overall hardness of the rubber sole. Appropriate hardness can provide sufficient support while maintaining sufficient elasticity to meet the needs of outdoor sports.

[0026] In a second aspect, the present application provides a method for preparing a rubber sole for outdoor sports, using the following technical solution: A method for preparing a rubber sole for outdoor sports, comprising the following preparation steps: S1, mixing rubber, ethylene-vinyl acetate copolymer and polyvinyl alcohol at a mixing temperature of 60-65° C. to obtain a mixture A; S2, mixing mixture A, abrasion resistant agent, a cross-linking agent and a foaming agent at a mixing temperature of 50-55° C. to obtain mixture B; S3, mixing mixture B, a vulcanizing agent and an accelerator at a mixing temperature of 45-50° C. to obtain a mixture C; S4, rolling the mixture C into a sheet, and then vulcanizing the sheet to obtain a rubber sole for outdoor sports, wherein the vulcanization molding temperature is 180-200° C., and the vulcanization time is 20-30 min.

[0027] By adopting the technical solution, the various raw materials can be fully mixed to obtain a rubber sole for outdoor sports with uniform pores, stable structure, good wear resistance and good elasticity.

[0028] In summary, this application has the following beneficial effects: 1. Enhanced pore structure: Ethylene-vinyl acetate copolymer can improve the flexibility and elasticity of the rubber matrix, and polyvinyl alcohol can improve the adhesion of the rubber. The two together with rubber can help form a more uniform and firmly connected pore structure during the foaming process, reduce the risk of pore rupture and deformation, and improve the shock absorption and support of the sole.

[0029] 2. Good wear resistance: The corundum, wollastonite and cellulose fiber powder in the wear-resistant agent can be evenly distributed in the rubber matrix to form a hard support point, so that the sole can resist wear when it is worn by the outside world and protect the rubber matrix from damage. At the same time, the three can also be evenly distributed in the rubber matrix to form a network structure, enhance the thickness and strength of the cell wall, prevent the cell from breaking and deformation, and extend the service life of the sole. DETAILED DESCRIPTION Example

[0030] The EPDM rubber was purchased from Dongguan Chengjin Plastic Chemical Co., Ltd. The brand is Korean SK and the grade is S5527F.

[0031] Butadiene rubber was purchased from Guangzhou Degao New Materials Co., Ltd. The brand is Korean LVE and the grade is K30AF.

[0032] Microcrystalline cellulose was purchased from Wuhan Jiyesheng Chemical Co., Ltd., and the implementation standard was the national standard.

[0033] The hemp fiber was purchased from Hualong Hemp Spinning Craft Products in Lu'an City. The grade was first-class and it needed to be crushed after purchase.

[0034] The viscose fiber was purchased from Hangzhou Yaoyang Technology Co., Ltd. with the product number yaoyang. It needed to be crushed after purchase.

[0035] Example 1 A rubber sole for outdoor sports is prepared by the following method: S1, 400 g of rubber, 150 g of ethylene-vinyl acetate copolymer and 300 g of polyvinyl alcohol were mixed at a mixing temperature of 60° C., a mixing time of 80 min and a mixing pressure of 12 MPa to obtain a mixture A; S2, the mixture A, 62g of anti-wear agent, 20g of cross-linking agent (diisopropylbenzene peroxide) and 50g of foaming agent (p-toluenesulfonyl hydrazide) were mixed at a mixing temperature of 50°C, a mixing time of 10min and a mixing pressure of 8MPa to obtain a mixture B; S3, mixing mixture B, 10 g of a vulcanizing agent (sulfur) and 8 g of an accelerator (2,2'-dibenzothiazyl disulfide) at a mixing temperature of 45° C., a mixing time of 3 min, and a mixing pressure of 10 MPa to obtain a mixture C; S4, rolling the mixture C into a sheet, and then vulcanizing the sheet to obtain a rubber sole for outdoor sports, wherein the vulcanization molding temperature is 180° C. and the vulcanization time is 20 min.

[0036] The wear-resistant agent is composed of corundum, wollastonite and cellulose fiber in a weight ratio of 2:3:1, the average particle size of the corundum is 20-50nm, the average particle size of the wollastonite is 100-150nm, and the average particle size of the cellulose fiber (microcrystalline cellulose) is 150-180nm.

[0037] The ethylene content in the ethylene-vinyl acetate copolymer is 20 wt % and the number average molecular weight is 15,000.

[0038] The number average molecular weight of polyvinyl alcohol is 25,000.

[0039] The difference between Example 2-3 and Example 1 is that the types of raw materials, amounts and experimental parameters for preparing rubber soles for outdoor sports are different. The specific differences are shown in Table 1: In Example 2, the wear-resistant agent is composed of corundum, wollastonite and cellulose fiber in a weight ratio of 2:3:1, the average particle size of corundum is 50-100nm, the average particle size of wollastonite is 150-250nm, and the average particle size of cellulose fiber (microcrystalline cellulose) is 180-220nm.

[0040] In Example 3, the wear-resistant agent is composed of corundum, wollastonite and cellulose fiber in a weight ratio of 2:3:1, the average particle size of corundum is 100-200nm, the average particle size of wollastonite is 250-300nm, and the average particle size of cellulose fiber (microcrystalline cellulose) is 180-250nm.

[0041] Example 4 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the wear-resistant agent is obtained by mixing corundum, wollastonite and cellulose fiber in a weight ratio of 3:2:1.

[0042] Example 5 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the wear-resistant agent is obtained by mixing corundum, wollastonite and cellulose fiber in a weight ratio of 1:3:2.

[0043] Example 6 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the wear-resistant agent is composed of corundum, wollastonite and cellulose fiber in a weight ratio of 2:3:1, the average particle size of the corundum is 20-50nm, the average particle size of the wollastonite is 20-50nm, and the average particle size of the cellulose fiber is 20-50nm.

[0044] Example 7 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the rubber is obtained by mixing EPDM rubber and butadiene rubber in a weight ratio of 8:3.

[0045] Example 8 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the rubber is obtained by mixing EPDM rubber and butadiene rubber in a weight ratio of 8:5.

[0046] Example 9 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the foaming agent is obtained by mixing p-toluenesulfonyl hydrazide and diisopropyl azodicarboxylate in a weight ratio of 1:0.8.

[0047] Example 10 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 7 is that the foaming agent is obtained by mixing p-toluenesulfonyl hydrazide and diisopropyl azodicarboxylate in a weight ratio of 2:0.8.

[0048] Embodiment 11 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the number average molecular weight of polyvinyl alcohol is 150,000.

[0049] Example 12 A rubber sole for outdoor sports. The difference between this embodiment and embodiment 1 is that the content of ethylene in the ethylene-vinyl acetate copolymer is 50wt%.

[0050] Comparative Example Comparative Example 1 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that the wear-resistant agent is silicon dioxide, and the silicon dioxide is obtained by mixing silicon dioxide with an average particle size of 20-50nm, silicon dioxide with an average particle size of 100-150nm, and silicon dioxide with an average particle size of 150-180nm in a weight ratio of 2:3:1.

[0051] Comparative Example 2 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that silicon dioxide is used instead of corundum.

[0052] Comparative Example 3 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that silicon dioxide is used instead of wollastonite.

[0053] Comparative Example 4 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that hydroxypropyl methylcellulose is used instead of cellulose fiber.

[0054] Polyester Comparative Example 5 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that polyurethane is used instead of ethylene-vinyl acetate copolymer.

[0055] Polyurethane was purchased from Dongguan Hongguohai Plastic Co., Ltd. The brand is BASF of Germany and the grade is 1198A.

[0056] Comparative Example 6 A rubber sole for outdoor sports. The difference between this comparative example and Example 1 is that hydroxypropyl methylcellulose is used instead of polyvinyl alcohol.

[0057] Detection method / test method Wear resistance test: The rubber soles for outdoor sports prepared in Examples 1-12 and Comparative Examples 1-6 were tested according to the test method in GB / T9867-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrasion machine method)".

[0058] Rebound resilience test: The rubber soles for outdoor sports prepared in Examples 1-12 and Comparative Examples 1-6 were tested according to the test method in GB / T16812009 "Determination of the rebound resilience of vulcanized rubber" using a rebound testing machine.

[0059] The anti-cracking performance test method is as follows: the rubber soles for outdoor sports prepared in Examples 1-12 and Comparative Examples 1-6 are placed in an oven at 70°C for 2 hours, taken out and placed in a freezer at -15°C for 2 hours, and then the process is repeated. The oven and freezer are placed in sequence as one cycle. After observing the cracking of each sole material after several cycles, the greater the number of cycles, the better the anti-cracking performance and the better the durability.

[0060] Tensile strength: tested in accordance with GB / T 10654-2001.

[0061] Hardness: Shore A hardness is tested according to ISO7619:1997. The experimental data is shown in Table 2: Table 2 Experimental data of Examples 1-12 and Comparative Examples 1-6 It can be seen from Examples 1-12 and Comparative Examples 1-6 in combination with Table 2 that the rubber soles for outdoor sports prepared by the formula in the present application have good wear resistance, elasticity, hardness, strength and durability.

[0062] By comparing Example 1 with Comparative Example 1, the wear resistance, resilience, crack resistance, tensile strength and hardness of the silicon dioxide used in Comparative Example 1 are greatly reduced; By comparing Example 1 with Comparative Examples 2-4, other materials are used in Comparative Examples 2-4 to replace corundum, wollastonite and cellulose fiber respectively, and the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles for outdoor sports are reduced; From the experimental data of Example 1 and Comparative Examples 1-4, the present application can further improve the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports by mixing corundum, wollastonite and cellulose fiber as wear-resistant agents.

[0063] Comparing Example 1 with Examples 4-5, the wear resistance and hardness of Example 4 are improved, but the resilience, crack resistance and tensile strength are slightly reduced; the resilience of Example 5 is improved, but the wear resistance, crack resistance, tensile strength and hardness are reduced, indicating that by optimizing the dosage of corundum, wollastonite and cellulose fiber, the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports can be comprehensively improved.

[0064] Comparing Example 1 with Example 6, the wear resistance, resilience, crack resistance, tensile strength and hardness in Example 6 are all reduced, indicating that optimizing the average particle size of corundum, the average particle size of wollastonite and the average particle size of cellulose fiber is beneficial to improving the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports.

[0065] Comparing Example 1 with Examples 7-8, the wear resistance, resilience, crack resistance, tensile strength and hardness of Examples 7-8 are all improved, indicating that by optimizing the type and amount of rubber, the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports can be further improved.

[0066] Comparing Example 1 with Example 9, the wear resistance, resilience, crack resistance, tensile strength and hardness of Example 8 are all improved; Comparing Example 7 with Example 10, the wear resistance, resilience, crack resistance, tensile strength and hardness of Example 9 are all improved; From the experimental results of Examples 1 and 9, 7 and 10, it can be seen that optimizing the type and amount of the foaming agent can help improve the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports.

[0067] Comparing Example 1 with Example 11, the wear resistance, resilience, crack resistance, tensile strength and hardness of Example 11 are slightly reduced, indicating that optimizing the number average molecular weight of polyvinyl alcohol is beneficial to improving the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports.

[0068] Comparing Example 1 with Example 12, the wear resistance, resilience, crack resistance, tensile strength and hardness of Example 12 are slightly reduced, indicating that optimizing the ethylene content in the ethylene-vinyl acetate copolymer is beneficial to improving the wear resistance, resilience, crack resistance, tensile strength and hardness of the rubber soles used for outdoor sports.

[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A rubber sole for outdoor sports. It is characterized in that Prepared from the following raw materials in weight percentage: Rubber 40-50% Ethylene-vinyl acetate copolymer 10-15% Polyvinyl alcohol 20-30% Crosslinking agent 1-2% Accelerator 0.3-0.8% Vulcanizing agent 0.5-1% Foaming agent 3-5% The rest is anti-wear agent The wear-resistant agent is obtained by mixing corundum, wollastonite and cellulose fiber.

2. A rubber sole for outdoor sports according to claim 1, Features: The weight ratio of the corundum, the wollastonite and the cellulose fiber is (2-5):(3-6):

1.

3. A rubber sole for outdoor sports according to claim 2, Features: The rubber is obtained by mixing EPDM rubber and butadiene rubber in a weight ratio of 8:(3-5).

4. The rubber sole for outdoor sports according to claim 1, Features: The average particle size of the corundum is 20-200 nm, the average particle size of the wollastonite is 100-300 nm, and the average particle size of the cellulose fiber is 150-250 nm.

5. A rubber sole for outdoor sports according to claim 4, Features: The foaming agent is obtained by mixing p-toluenesulfonyl hydrazide and diisopropyl azodicarboxylate in a weight ratio of (1-2):0.

8.

6. The rubber sole for outdoor sports according to claim 4, Features: The number average molecular weight of the polyvinyl alcohol is 25,000-120,000.

7. The rubber sole for outdoor sports according to claim 1, Features: The content of ethylene in the ethylene-vinyl acetate copolymer is 20-40wt%.

8. The rubber sole for outdoor sports according to claim 1, Features: The cross-linking agent is one of dicumyl peroxide, 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane or benzoyl peroxide.

9. The rubber sole for outdoor sports according to claim 1, Features: The vulcanizing agent is one of sulfur or triallyl isocyanurate.

10. A method for preparing a rubber sole for outdoor sports as claimed in any one of claims 1 to 9, It is characterized in that The method comprises the following preparation steps: S1, mixing rubber, ethylene-vinyl acetate copolymer and polyvinyl alcohol at a mixing temperature of 60-65° C. to obtain a mixture A; S2, mixing mixture A, abrasion resistant agent, a cross-linking agent and a foaming agent at a mixing temperature of 50-55° C. to obtain mixture B; S3, mixing mixture B, a vulcanizing agent and an accelerator at a mixing temperature of 45-50° C. to obtain a mixture C; S4, rolling the mixture C into a sheet, and then vulcanizing the sheet to obtain a rubber sole for outdoor sports, wherein the vulcanization molding temperature is 180-200° C., and the vulcanization time is 20-30 min.

Citation Information

Patent Citations

  • Non-gumming wear-resistant sole and preparation method thereof

    CN109370037A

  • High-mechanical-strength wear-resistant EVA composite foam material and preparation method thereof

    CN111333950A

  • Lightweight and wear-resistant rubber foamed sole, preparation method thereof and sports shoe

    CN113372624A

  • Wear-resistant sole and preparation process thereof

    CN115558191A

  • Wear-resistant high polymer material and preparation method thereof

    CN118562280A