Black pigment for preparing polyurethane thin coating film as well as preparation and application methods thereof
Through the combination of graphene oxide and nano-scale carbon black black, the problems of uneven dispersion and insufficient light transmittance during thin coating are solved, and the uniformity and high light transmittance of the polyurethane film are achieved, which improves mechanics and resistance Thermal performance is suitable for the protection of electronic equipment screens, and the process is environmentally friendly and safe.
Patent Information
- Application Number
- CN202411350366.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
During the thin coating process, existing nano-grade black pigments have problems such as complex preparation process, unsuitable thin coating, and uneven film color, making it difficult to achieve uniform dispersion and high light transmittance in water-based polyurethane thin coating films.
The black pigment combined with graphene oxide and nano-scale carbon black is used to react with aqueous polyurethane through the reaction of carboxyl, hydroxyl and other groups of graphene oxide to achieve uniform dispersion of carbon black and is connected through carbon-carbon π-π conjugated bonds. , combined with physical adsorption and chemical reactions, a stable composite film is formed.
It realizes the uniform black spots and particles-free of polyurethane films, adjustable light transmittance, and improves mechanical strength and heat resistance. It is suitable for the protection of electronic equipment screens. The process is suitable for water-based conditions and does not require the addition of organic solvents, which is environmentally friendly and safe.
Smart Images

Figure BDA0005062183240000131 
Figure BDA0005062183240000141 
Figure BDA0005062183240000151
Abstract
Description
Technical Field
[0001] The invention relates to a black pigment for preparing a polyurethane thin coating film and a preparation and application method thereof, belonging to the technical field of thin coating pigment preparation. Background Art
[0002] At present, with the popularization of electronic products, electronic components play a pivotal role in them, and have received more and more attention, and related industries are gradually emerging. The application of black pigments in coatings is mainly reflected in providing color, hiding power, mechanical strength and specific functionality.
[0003] Black pigments, such as carbon black, are used as coloring pigments in inks, paints, coatings, plastics and other products. They not only make the coating film appear colorful, but also give the coating film a certain color, increase the volume of the coating film, and make it have a certain ability to cover the base layer, thereby improving the mechanical strength of the coating film.
[0004] In coatings, the application of black pigments is not limited to providing basic color requirements, but also involves improving various physical and chemical properties of the coating film. For example, the use of pigment carbon black can make the coating film have a better ability to cover the coated object and play its decorative and protective role. At the same time, by adding specific black pigments, such as black iron oxide, the durability and corrosion resistance of the coating film can be further improved, protecting the coating base layer and resisting the erosion of various corrosive substances.
[0005] The Chinese invention patent with patent number CN101492585A discloses a stable black nanometer aqueous pigment dispersion, which has the characteristics of excellent dispersibility and storage stability. The dispersion prevents the pigment particles from agglomerating by anchoring the dispersant to the surface of the pigment particles, thereby increasing stability. However, in this patent, high shear, cyclic grinding and dispersion are required, and inkjet is required. Not only is the process route complicated and time-consuming, but the invention is not suitable for thin coating and cannot achieve the characteristic of uniform thin coating.
[0006] The following problems are common in the current nano-scale black pigment preparation technology, including complex preparation process, only suitable for thick coating, thin coating has particles and black spots, uneven film color and other problems. As a pigment used in water-based polyurethane resin, thin coating film is used to form a protective film on LED electronic screens, not only must the current system be stable and uniformly dispersed, but also there must be no particles and black spots during the thin coating process, and the overall film must be uniform.
[0007] In view of the above-mentioned defects, the present invention aims to create a black pigment for preparing a polyurethane thin coating film and a preparation and application method thereof, so as to make it more valuable for industrial use. Summary of the invention
[0008] In order to solve the above technical problems, the purpose of the present invention is to provide a black pigment for preparing a polyurethane thin coating film and a preparation and application method thereof.
[0009] The black pigment for preparing a polyurethane thin coating film of the present invention comprises the following substances in parts by weight:
[0010] 3-15 parts of black pigment;
[0011] 20-25 parts of waterborne polyurethane;
[0012] The solid content of carbon black in the black pigment is 2%, and the solid content of graphene oxide is 2%;
[0013] The dry weight of the graphene oxide accounts for 1 to 5% of the dry weight of the waterborne epoxy resin;
[0014] The dry weight of the carbon black accounts for 1-5% of the dry weight of the waterborne epoxy resin.
[0015] The light transmittance of the film after thin coating can be adjusted in a wide range, the surface is uniform and free of black spots and particles, the mechanical strength and heat resistance are excellent, and the overall performance first increases with the increase of the amount of black pigment, and then there is an unobvious trend of improvement. By adjusting the dry weight ratio of graphene oxide and carbon black in the aqueous polyurethane solution, the light transmittance of the film can be adjusted. The blank sample has a maximum light transmittance of 85.8%, and the minimum is 14.7% after adding pigment. The use of this black pigment compounded with graphene oxide and carbon black can adjust the light transmittance of the polyurethane film to a large range, so it is widely used and meets the protection requirements for the screens of electronic devices.
[0016] Furthermore, the black pigment comprises the following substances by weight:
[0017] 10-12 parts of carbon black dispersion;
[0018] 40-45 parts of homogeneous graphene oxide dispersion;
[0019] The particle size of graphene oxide in the homogeneous graphene oxide dispersion is 2-3 μm.
[0020] The black pigment of the present invention needs to meet the black performance in addition to thin coating. In the process of coating, the single carbon black will have black spots and particles in the case of thin coating because of the poor dispersion effect in water; while graphene oxide has no black spots and no particles, its color is yellowish, especially affecting its use in terms of optical performance; graphene oxide has abundant carboxyl groups on its edges and many hydroxyl groups, carbonyl groups, epoxy groups, etc. on its surface. Waterborne polyurethane is synthesized from isocyanate and polyol, so the alcohol on the polyurethane can react with it, so that graphene oxide and waterborne polyurethane can be connected together by chemical bonds. Graphene oxide and carbon black have relatively strong adsorption capacity, graphene oxide sheets are relatively large, and the carbon black selected by the present invention is nanometer-level. The effect of carbon black itself being dispersed in water is not good, but graphene oxide has a very good dispersion effect in water because it has many groups such as carboxyl groups and hydroxyl groups, so after carbon black is adsorbed on graphene oxide, carbon black is uniformly dispersed in the graphene oxide aqueous solution. The adsorption method of carbon black and graphene oxide is to connect through the π-π conjugated bond generated between carbon and carbon and maintain stability. Graphene oxide plays the role of a bridge dispersant in this technical solution. On the one hand, it can adsorb carbon black through physical methods to achieve color change, and on the other hand, it can react chemically with water-based polyurethane to allow the water-based polyurethane to wrap the graphene oxide sheet to achieve the effect of adhesion.
[0021] Carbon black itself is insoluble in water. If graphene oxide is removed and carbon black is directly added to waterborne polyurethane, the two will have no binding force, which will cause black spots and particles to appear on the surface of the carbon black-polyurethane film. Therefore, GO is needed as a dispersant to help carbon black disperse better in water. The two complement each other to achieve thin coating. The reason why carbon black-GO-WPU can be coated thinly is that other coatings will produce black spots or particles when coated thinly, and these black spots or black particles will be covered when coated thickly, making them invisible to the naked eye. When the coating is thinned to 1-2μm, they will emerge. However, in the carbon black-GO-WPU method, the black film coated is uniform, without black spots or particles, and has a corresponding light transmittance regardless of thickness.
[0022] Further, the carbon black dispersion is prepared by the following scheme:
[0023] 40-45 parts of deionized water were weighed by weight, 4-4.5 parts of dispersant BYK2013 were added, and the mixture was stirred at 500 rpm with a magnetic stirrer for 10 min. Then, 6.6-6.7 parts of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 500-1000 nm were added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion.
[0024] The technical solution provided by the present invention is suitable for use under aqueous conditions, does not require the addition of organic solvents, and is environmentally friendly and safe. Under this technical solution, the standard for judging whether a thin coating can be applied is that the coating has no black spots or particles and has a good optical effect, and is uniform and integrated when observed with the naked eye, and it is not simply whether the film can be coated with a thickness of 2-3 μm.
[0025] Furthermore, the homogeneous graphene oxide dispersion is prepared by the following scheme:
[0026] (1) taking graphene oxide, dispersing it in water while stirring, the stirring speed is 200 rpm, the stirring and dispersing time is 1 hour, and a graphene oxide dispersion with a solid content of 5% is prepared;
[0027] (2) Ammonia water was added to the above graphene oxide dispersion to adjust the pH of the dispersion to 7, and the dispersion was passed through a homogenizer and homogenized 2 to 3 times under a pressure of 80 MPa to finally obtain a homogeneous graphene oxide dispersion with a graphene oxide particle size of 2 to 3 μm.
[0028] In addition to the dispersing effect, the addition of graphene oxide in the technical solution of the present invention can also serve as a bridge structure to improve the interface interaction between the additive and the waterborne polyurethane matrix, so that the graphene oxide sheet is more closely connected with the waterborne polyurethane, reducing the problem of decreased mechanical properties of the composite film due to stress concentration, and improving the tensile strength of the thin coating film;
[0029] In addition, because graphene oxide has a large specific surface area, small particle size, and contains many oxygen-containing groups, it increases the probability of chemical or physical bonding with waterborne polyurethane, causing it to be disorderly arranged in the thin film to form a complex network-type heat dissipation structure. At the same time, the hydrogen bonds between graphene oxide and the carbamate group inhibit the thermal decomposition of the film to a certain extent, thereby improving the heat resistance of the thin-coated blend film.
[0030] A method for preparing a black pigment for preparing a polyurethane thin coating film, characterized in that the specific preparation steps are:
[0031] According to weight, 10 to 12 parts of carbon black dispersion and 40 to 45 parts of homogeneous graphene oxide dispersion are weighed, water is added and mixed, and stirred evenly with a dispersion disk, the stirring speed is controlled to 2000 rpm, and stirring is carried out for 30 to 40 minutes; in the final black pigment, the solid content of carbon black is 2%, and the solid content of graphene oxide is 2%.
[0032] The application method of the black pigment for preparing the polyurethane thin coating film comprises the following specific application steps:
[0033] 3 to 15 parts of black pigment were weighed by weight and added to 20 to 25 parts of waterborne polyurethane. The mixture was stirred at 1000 rpm with a magnetic stirrer for 30 min to disperse evenly. The mixture was allowed to stand for 1 h to defoam. A sample was taken onto a PET substrate with a dropper and coated with a 25 μm wire rod. The film was placed in an oven at 80°C for 1 min to obtain a polyurethane film.
[0034] Furthermore, the polyurethane film has a thickness of 2-3 μm.
[0035] By means of the above scheme, the present invention has at least the following advantages:
[0036] (1) The black pigment of the present invention needs to meet the black performance requirements in addition to being applied thinly. Carbon black alone will produce black spots and particles in the thin coating process because of its poor dispersion effect in water. Although graphene oxide has no black spots and no particles, its color is yellowish, which affects its use, especially in terms of optical performance. Graphene oxide has abundant carboxyl groups on its edges and many hydroxyl groups, carbonyl groups, epoxy groups, etc. on its surface. Waterborne polyurethane is synthesized from isocyanate and polyol, so the alcohol on the polyurethane can react with it, so that graphene oxide and waterborne polyurethane can be connected together through chemical bonds. Graphene oxide and carbon black have relatively strong adsorption capacity. Graphene oxide sheets are relatively large, while the carbon black selected in the present invention is nano-scale. The effect of carbon black itself being dispersed in water is not good, but graphene oxide has a very good dispersion effect in water because it has many carboxyl groups, hydroxyl groups, etc., so after carbon black is adsorbed on graphene oxide, carbon black is evenly dispersed in the graphene oxide aqueous solution. The adsorption method of carbon black and graphene oxide is to connect through the π-π conjugated bond generated between carbon and carbon and maintain stability. Graphene oxide plays the role of a bridge dispersant in this technical solution. On the one hand, it can adsorb carbon black through physical methods to achieve color change, and on the other hand, it can react chemically with water-based polyurethane to allow the water-based polyurethane to wrap the graphene oxide sheet to achieve the effect of adhesion.
[0037] (2) Carbon black itself is insoluble in water. If graphene oxide is removed and carbon black is directly added to waterborne polyurethane, the two will have no binding force, which will cause black spots and particles to appear on the surface of the carbon black-polyurethane film. Therefore, GO is needed as a dispersant to help carbon black disperse better in water. The two complement each other to achieve thin coating. The reason why carbon black-GO-WPU can be coated thinly is that other coatings will produce black spots or particles when coated thinly, and these black spots or black particles will be covered when coated thickly, making them invisible to the naked eye. When the coating is thinned to 1-2μm, they will emerge. However, under the method of carbon black-GO-WPU, the black film coated is uniform, free of black spots and particles, and has a corresponding light transmittance regardless of thickness.
[0038] (3) The technical solution provided by the present invention is suitable for use under aqueous conditions, does not require the addition of organic solvents, and is environmentally friendly and safe. Under this technical solution, the criterion for judging whether a thin coating can be applied is that the coating has no black spots or particles and has a good optical effect, and is uniform and integrated when observed with the naked eye, rather than simply whether the film can be coated with a thickness of 2-3 μm.
[0039] (4) In addition to the dispersing effect, the addition of graphene oxide in the technical solution of the present invention can also serve as a bridge structure to improve the interfacial interaction between the additive and the waterborne polyurethane matrix, so that the graphene oxide sheet is more closely connected to the waterborne polyurethane, reducing the problem of decreased mechanical properties of the composite film due to stress concentration, and improving the tensile strength of the thin coating film;
[0040] (5) In addition, because graphene oxide has a large specific surface area, a small particle size, and contains many oxygen-containing groups, it increases the probability of chemical or physical bonding with waterborne polyurethane, causing it to be disorderly arranged in the thin film to form a complex network-type heat dissipation structure. At the same time, the hydrogen bonds between graphene oxide and the carbamate group inhibit the thermal decomposition of the film to a certain extent, thereby improving the heat resistance of the thin-film blend.
[0041] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION
[0042] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0043] A method for preparing a black pigment for preparing a polyurethane thin coating film comprises the following steps:
[0044] raw material:
[0045] Graphene oxide, using SE243PPW model product of Changzhou Sixth Element Materials Technology Co., Ltd.;
[0046] Pigment carbon black, S series S24061501 batch carbon black from Wuxi Tyco Nano New Materials Co., Ltd.
[0047] As the dispersant, BYK2013 dispersant produced by German BYK Chemical was selected.
[0048] (1) preparing a homogeneous graphene oxide dispersion: taking graphene oxide, dispersing it in water while stirring, the stirring speed is 200 rpm, the stirring and dispersing time is 1 hour, and a graphene oxide dispersion with a solid content of 5% is obtained;
[0049] Adding ammonia water to the above graphene oxide dispersion to adjust the pH of the dispersion to 7, passing the dispersion through a homogenizer, and homogenizing 2 to 3 times under a pressure of 80 MPa to finally obtain a homogeneous graphene oxide dispersion with a graphene oxide particle size of 2 to 3 μm;
[0050] (2) Preparation of carbon black dispersion: 40-45 parts by weight of deionized water were weighed, 4-4.5 parts of dispersant BYK2013 were added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer, and then 6.6-6.7 parts of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 500-1000 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion;
[0051] (3) Preparation of black pigment: 10 to 12 parts by weight of carbon black dispersion and 40 to 45 parts of homogeneous graphene oxide dispersion were weighed, water was added and mixed, and stirred evenly with a dispersion disk, the stirring speed was controlled to 2000 rpm, and the stirring was performed for 30 to 40 minutes; the final black pigment had a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0052] (4) Application method of black pigment for preparing polyurethane thin coating film: weigh 3 to 15 parts of black pigment by weight, add it to 20 to 25 parts of water-based polyurethane, use a magnetic stirrer to stir at a speed of 1000 rpm for 30 minutes to disperse evenly, and let it stand for 1 hour to defoam; use a dropper to take a sample onto a PET substrate, use a 25 μm wire rod to coat the film, and place the film in an oven at 80°C for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3 μm.
[0053] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0054] Example 1
[0055] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0056] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 500 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0057] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0058] (4) Application method of black pigment for preparing polyurethane thin coating film: weigh 3 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to apply the film, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.06g, the dry weight of carbon black is 0.06g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 2% of the polyurethane
[0059] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0060] Example 2
[0061] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0062] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 600 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0063] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0064] (4) Application method of black pigment for preparing polyurethane thin coating film: weigh 6 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to apply the film, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.12g, the dry weight of carbon black is 0.12g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 4% of the polyurethane
[0065] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0066] Example 3
[0067] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0068] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 700 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0069] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0070] (4) Application method of black pigment for preparing polyurethane thin coating film: weigh 9 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to apply the film, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.18g, the dry weight of carbon black is 0.18g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 6% of the polyurethane
[0071] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0072] Example 4
[0073] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0074] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 800 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0075] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0076] (4) Application method of black pigment for preparing polyurethane thin coating: weigh 12 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to apply the film, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.24g, the dry weight of carbon black is 0.24g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 8% of the polyurethane
[0077] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0078] Example 5
[0079] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0080] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 1000 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0081] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0082] (4) Application method of black pigment for preparing polyurethane thin coating: weigh 15 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to apply the film, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.30g, the dry weight of carbon black is 0.30g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 10% of the polyurethane
[0083] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0084] Example 6
[0085] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0086] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 1000 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0087] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0088] (4) Application method of black pigment for preparing polyurethane thin coating film: weigh 20g black pigment, add it to 20g waterborne polyurethane, stir it with a magnetic stirrer at 1000rpm for 30min to disperse it evenly, and let it stand for 1h to defoam; use a dropper to sample it on a PET substrate, use a 25μm wire rod to coat it, and put the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.40g, the dry weight of carbon black is 0.40g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 15% of the polyurethane.
[0089] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0090] Example 7
[0091] (1) preparing a homogeneous graphene oxide dispersion: taking 10 g of a graphene oxide filter cake having a solid content of 42.89%, breaking it into small pieces, and dispersing it in 75.78 g of water while stirring, at a speed of 200 rpm, for 1 hour, to prepare a graphene oxide aqueous dispersion having a solid content of 5%; adding ammonia water to the graphene oxide dispersion until the pH of the dispersion reaches 7; passing the dispersion through a homogenizer, homogenizing it twice at a pressure of 80 MPa, and finally obtaining a homogeneous graphene oxide dispersion, wherein the particle size of the graphene oxide is 2-3 μm, and retaining a sample for later use;
[0092] (2) Preparation of carbon black dispersion: 49.33 g of deionized water was weighed, 4 g of dispersant BYK2013 was added, and the mixture was stirred at 500 rpm for 10 min using a magnetic stirrer. Then, 6.67 g of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 500 nm was added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion for later use;
[0093] (3) Preparation of black pigment: Take 10 g of carbon black dispersion and 40 g of homogeneous graphene oxide dispersion, mix and stir evenly with a dispersion disk, add water and mix and stir evenly with a dispersion disk, control the stirring speed to 2000 rpm, and stir for 30 to 40 minutes; the final black pigment has a carbon black solid content of 2% and a graphene oxide solid content of 2%.
[0094] (4) Application method of black pigment for preparing polyurethane thin coating: weigh 2 grams of black pigment, add it to 20 grams of waterborne polyurethane, stir it with a magnetic stirrer at a speed of 1000 rpm for 30 minutes to disperse it evenly, and let it stand for 1 hour to defoam; use a dropper to sample it on a PET substrate, apply the film with a 25μm wire rod, and bake the film in an oven at 80℃ for 1 minute to obtain a polyurethane film with a smooth surface, uniform and particle-free, and a film thickness of 2-3μm. The dry weight of graphene oxide in the solution is 0.04g, the dry weight of carbon black is 0.04g, and the dry weight of polyurethane is 6g, that is, the dry weight of the composite liquid accounts for 1.5% of the polyurethane;
[0095] (5) Performance test: Use WH-100 haze meter to test the light transmittance, the test standard is GB / T2410-08.
[0096] Comparative Example 1
[0097] The preparation method of the polyurethane film in this comparative example is the same as that in Example 3, except that only water-based polyurethane is used without adding the black pigment of the present invention.
[0098] Comparative Example 2
[0099] The preparation method of the modified polyurethane protective film in this control example is the same as that in Example 3, except that 3.6 g of the graphene oxide dispersion with a solid content of 5% prepared in step 1 is added to 20 g of waterborne polyurethane, the dry weight of graphene oxide is 0.18 g, and the dry weight of waterborne epoxy resin is 6 g, that is, the dry weight of graphene oxide accounts for 3% of the dry weight of waterborne epoxy resin.
[0100] Comparative Example 3
[0101] The preparation method of the modified polyurethane protective film in this control example is the same as that in Example 3, except that 4.56 g of the carbon black dispersion with a solid content of 3.9% prepared in step 2 is added to 20 g of waterborne polyurethane, the dry weight of carbon black is 0.18 g, and the dry weight of waterborne epoxy resin is 6 g, that is, the dry weight of carbon black accounts for 3% of the dry weight of waterborne epoxy resin.
[0102] The performance of Examples 1-7 and Comparative Examples 1-3 of the present invention were tested respectively, and the test results are shown in Table 1:
[0103] Detection method:
[0104] Light transmittance: Use WH-100 haze meter to test light transmittance, the test standard is GB / T 2410-08;
[0105] Tensile strength: tested using a universal mechanical testing machine;
[0106] Thermal decomposition temperature: tested by differential scanning calorimeter (DSC);
[0107] Table 1 Test results of light transmittance of modified polyurethane protective film at different compound liquid addition amounts
[0108]
[0109]
[0110]
[0111] It can be seen from the test data in the above table that in Examples 1-5 of the present invention, the film finally prepared by the black pigment coating used to prepare the polyurethane thin coating can achieve thin coating, and the light transmittance of the film after thin coating can be adjusted in a wide range, the surface is uniform without black spots and particles, the mechanical strength and heat resistance are very excellent, and the overall performance is first in an increasing state, and the subsequent improvement is not obvious. The light transmittance of the film can be adjusted by adjusting the dry weight ratio of graphene oxide and carbon black in the aqueous polyurethane solution. The blank sample has the highest light transmittance of 85.8%, and the lowest after adding pigment is 14.7%. Using this black pigment compounded with graphene oxide and carbon black, the light transmittance of the polyurethane film can be adjusted to a large span, so it is widely used and meets the protection requirements for the screen of electronic equipment.
[0112] In addition, in Examples 6 and 7, since the addition range of the black pigment exceeds the preferred addition range of the present invention, some performances are reduced, while the other performances are almost unchanged with the addition of the pigment amount. It can be confirmed that the addition amount of the black pigment of the present invention has an optimal range during use, and it is also confirmed that the technical solution of the present application is highly feasible, and it is confirmed that the black pigment of the present invention needs to meet the black performance in addition to thin coating. In the film coating process, the single carbon black will appear black spots and particles in the case of thin coating due to poor dispersion effect in water; while graphene oxide has no black spots and no particles, but the color is yellowish, especially affecting the use in terms of optical properties; graphene oxide has abundant carboxyl groups on the edge, and has many hydroxyl groups, carbonyl groups, epoxy groups, etc. on the surface. Waterborne polyurethane is synthesized from isocyanate and polyol, so the alcohol on the polyurethane can react with it, so that graphene oxide and waterborne polyurethane can be connected together by chemical bonds. Graphene oxide and carbon black have relatively strong adsorption capacity, graphene oxide flakes are relatively large, and the carbon black selected in the present invention is nanometer-level. Carbon black itself is not very effective in dispersing in water, but graphene oxide has a very good dispersing effect in water because it has many carboxyl groups, hydroxyl groups and other groups. Therefore, after carbon black is adsorbed on graphene oxide, carbon black is evenly dispersed in the graphene oxide aqueous solution. The adsorption method of carbon black and graphene oxide is connected by the π-π conjugated bond generated between carbon and carbon and can remain stable. Graphene oxide plays a bridging role as a dispersant in this technical solution. On the one hand, it can adsorb carbon black by physical methods to achieve color changes, and on the other hand, it can react chemically with water-based polyurethane to allow the water-based polyurethane to wrap the graphene oxide sheets to achieve the effect of adhesion.
[0113] Carbon black itself is insoluble in water. If graphene oxide is removed and carbon black is directly added to waterborne polyurethane, the two will have no binding force, which will cause black spots and particles to appear on the surface of the carbon black-polyurethane film. Therefore, GO is needed as a dispersant to help carbon black disperse better in water. The two complement each other to achieve thin coating. The reason why carbon black-GO-WPU can be coated thinly is that other coatings will produce black spots or particles when coated thinly, and these black spots or black particles will be covered when coated thickly, making them invisible to the naked eye. When the coating is thinned to 1-2μm, they will emerge. However, in the carbon black-GO-WPU method, the black film coated is uniform, without black spots or particles, and has a corresponding light transmittance regardless of thickness.
[0114] Moreover, the technical solution provided by the present invention is suitable for use under aqueous conditions, does not require the addition of organic solvents, and is environmentally friendly and safe. Under this technical solution, the criterion for judging whether a thin coating can be applied is that the coating has no black spots or particles and has a good optical effect, and is uniform and integrated when observed with the naked eye, and it is not simply whether the film can be coated with a thickness of 2-3 μm.
[0115] According to the coating results of Example 3, Comparative Example 2 and Comparative Example 3, the use of black pigments compounded with graphene oxide and carbon black is mainly due to the fact that the glue coating prepared by mixing graphene oxide with waterborne polyurethane is smooth and uniform without black spots or particles, and the coated film is yellowish, which affects the visual experience; the glue prepared by mixing high-pigment carbon black slurry with waterborne polyurethane will have a large number of particles and black spots on the surface after the coating is thin. The use of black pigments compounded with graphene oxide and carbon black can optimally avoid the problems of yellowish film color and black spot particles, and prepare waterborne polyurethane glue suitable for thin coating.
[0116] At the same time, the mechanical properties and heat resistance of the thin film without graphite oxide are significantly reduced, which can also prove that the addition of graphene oxide in the technical solution of the present invention can not only disperse, but also serve as a bridge structure to improve the interface interaction between the additive and the waterborne polyurethane matrix, so that the graphene oxide sheet is more closely connected with the waterborne polyurethane, reducing the problem of decreased mechanical properties of the composite film due to stress concentration, and improving the tensile strength of the thin film;
[0117] In addition, because graphene oxide has a large specific surface area, small particle size, and contains many oxygen-containing groups, it increases the probability of chemical or physical bonding with waterborne polyurethane, causing it to be disorderly arranged in the thin film to form a complex network-type heat dissipation structure. At the same time, the hydrogen bonds between graphene oxide and the carbamate group inhibit the thermal decomposition of the film to a certain extent, thereby improving the heat resistance of the thin-coated blend film.
[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A black pigment for preparing a polyurethane thin coating film, characterized in that: The following substances are included by weight: 3-15 parts of black pigment; 20-25 parts of waterborne polyurethane; The solid content of carbon black in the black pigment is 2%, and the solid content of graphene oxide is 2%; The dry weight of the graphene oxide accounts for 1 to 5% of the dry weight of the waterborne epoxy resin; The dry weight of the carbon black accounts for 1-5% of the dry weight of the waterborne epoxy resin.
2. The black pigment for preparing a polyurethane thin coating according to claim 1, characterized in that: The black pigment comprises the following substances by weight: 10-12 parts of carbon black dispersion; 40-45 parts of homogeneous graphene oxide dispersion; The particle size of graphene oxide in the homogeneous graphene oxide dispersion is 2-3 μm.
3. The black pigment for preparing a polyurethane thin coating according to claim 2, characterized in that: The carbon black dispersion is prepared by the following scheme: 40-45 parts of deionized water were weighed by weight, 4-4.5 parts of dispersant BYK2013 were added, and the mixture was stirred at 500 rpm with a magnetic stirrer for 10 min. Then, 6.6-6.7 parts of pigment carbon black slurry S24061501 with a mass fraction of 30% and a particle size of 500-1000 nm were added, and the mixture was stirred at 500 rpm for 10 min to obtain a carbon black dispersion.
4. The black pigment for preparing a polyurethane thin coating according to claim 2, characterized in that: The homogeneous graphene oxide dispersion is prepared by the following scheme: (1) taking graphene oxide, dispersing it in water while stirring, the stirring speed is 200 rpm, the stirring and dispersing time is 1 hour, and a graphene oxide dispersion with a solid content of 5% is prepared; (2) Ammonia water was added to the above graphene oxide dispersion to adjust the pH of the dispersion to 7, and the dispersion was passed through a homogenizer and homogenized 2 to 3 times under a pressure of 80 MPa to finally obtain a homogeneous graphene oxide dispersion with a graphene oxide particle size of 2 to 3 μm.
5. A method for preparing a black pigment for preparing a polyurethane thin coating as claimed in claim 1, characterized in that The specific preparation steps are: According to weight, 10 to 12 parts of carbon black dispersion and 40 to 45 parts of homogeneous graphene oxide dispersion are weighed, water is added and mixed, and stirred evenly with a dispersion disk, the stirring speed is controlled to 2000 rpm, and stirring is carried out for 30 to 40 minutes; in the final black pigment, the solid content of carbon black is 2%, and the solid content of graphene oxide is 2%.
6. The method for applying a black pigment for preparing a polyurethane thin coating according to any one of claims 1 to 5, characterized in that The specific application steps are: 3 to 15 parts of black pigment were weighed by weight and added to 20 to 25 parts of waterborne polyurethane. The mixture was stirred at 1000 rpm with a magnetic stirrer for 30 min to disperse evenly. The mixture was allowed to stand for 1 h to defoam. A sample was taken onto a PET substrate with a dropper and coated with a 25 μm wire rod. The film was placed in an oven at 80°C for 1 min to obtain a polyurethane film.
7. The method for applying a black pigment for preparing a polyurethane thin coating according to claim 6, characterized in that: The polyurethane film has a thickness of 2-3 μm.