Cracking-resistant high-adhesive-force ultraviolet curing coating and preparation method thereof
By using specific monomer combinations and fillers in UV curing coatings, the viscosity and surface tension are optimized, and the problems of crack resistance and insufficient adhesion of the coating are solved, and good construction effect and environmental protection are achieved, reducing the influence of color difference and human factors. .
Patent Information
- Application Number
- CN202411206956.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Existing ultraviolet curing coatings have poor performance in terms of crack resistance and high adhesion, and have color aberration problems, which affects construction effect and environmental protection.
Use monomer combinations such as trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and add silica, micropowder wax and alumina. Fillers, through a specific stirring step and combination of initiators, optimize viscosity and surface tension, and improve the gloss and scratch resistance of the coating.
The coating that achieves matching viscosity and surface tension is optimized, the coating effect is reduced, the influence of human factors is reduced, the wear resistance and gloss of the coating is improved, and the environmental protection and health of the product is ensured.
Smart Images

Figure BDA0005019294870000051 
Figure BDA0005019294870000061 
Figure BDA0005019294870000081
Abstract
Description
Technical Field
[0001] The invention relates to a crack-resistant and high-adhesion ultraviolet curing coating and a preparation method thereof, and relates to C09D, and in particular to the field of coating compositions. Background Art
[0002] As people pay more and more attention to environmental protection and health, the coatings used in furniture and other decoration industries for a long time are mostly PU or PE coatings, which have a high degree of pollution and will affect the health of construction workers. The preparation of photocurable coatings is green and environmentally friendly, low-cost, and easy to operate mechanically. Existing coatings for protecting furniture are mostly surface paint products. Although they are cheap, the coating surface is not scratch-resistant and the wear resistance of the coating is poor. Especially for the surface coating of paint products, spraying them on the surface of wooden furniture will produce color difference, reduce the construction effect, and cause the color of wooden furniture to be unnatural. Therefore, it is very important to develop a green and environmentally friendly photocurable coating with excellent construction effect.
[0003] Chinese invention patent CN201511007830.8 discloses a UV curing protective coating and its preparation method, which uses a certain weight ratio of acrylate resin, acrylate monomer, citrate, photoinitiator, and demolding aid, and is dispersed and mixed evenly. When used, the UV curing protective coating of the present invention is applied to the surface of the object to be protected, and is cured by ultraviolet irradiation to form a protective film. The coating achieves a strong adhesion effect, but there is a certain color difference when used. Chinese invention patent CN201811573437.9 discloses a high-toughness epoxy powder coating, which uses bisphenol A epoxy resin and hyperbranched polyamide resin to work together to achieve high toughness and high adhesion. However, there is color difference after construction, and the use effect is not good. Summary of the invention
[0004] In order to improve the crack resistance and high adhesion performance of UV-curing coatings, the first aspect of the present invention provides a UV-curing coating with crack resistance and high adhesion. The preparation raw materials include, by weight: 45-70 parts of a monomer combination, 1-10 parts of a copolymer amine acrylic resin, 0.1-2 parts of a mixed high molecular polymer, 0.1-4 parts of an acrylic copolymer solution, 0.1-2 parts of a dispersant, 5-20 parts of an initiator, 20-40 parts of a modified acrylate, and 10-20 parts of a solid filler.
[0005] As a preferred embodiment, the preparation raw materials include, by weight: 50-65 parts of monomer combination, 1-5 parts of copolymer amine acrylic resin, 0.1-0.5 parts of mixed high molecular polymer, 0.1-0.5 parts of acrylic copolymer solution, 0.1-0.5 parts of dispersant, 5-10 parts of initiator, 20-30 parts of modified acrylate, and 11-16 parts of solid filler.
[0006] As a preferred embodiment, the raw materials for preparation include, by weight: 57 parts of monomer combination, 2 parts of copolymer amine acrylic resin, 0.5 parts of mixed high molecular polymer, 0.5 parts of acrylic copolymer solution, 0.5 parts of dispersant, 6 parts of initiator, 26 parts of modified acrylate, and 11 parts of solid filler.
[0007] As a preferred embodiment, the modified acrylate is selected from one or a combination of epoxy acrylate, polyester acrylate, polyurethane acrylate, and silicone-modified acrylate.
[0008] As a preferred embodiment, the monomer combination is selected from one or a combination of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate.
[0009] As a preferred embodiment, the monomer combination is a combination of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate; preferably, the weight ratio of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate is (30-55): (10-35): (10-30): (5-15): (5-15).
[0010] As a preferred embodiment, the weight ratio of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate and glycidyl methacrylate is (15-20):(10-15):(10-20):(8-10):(8-10).
[0011] As a preferred embodiment, the weight ratio of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate is 15:12:10:10:10.
[0012] As a preferred embodiment, the solid filler is selected from one or a combination of silicon dioxide, micronized wax, aluminum oxide, talc, and calcium carbonate.
[0013] As a preferred embodiment, the solid filler is a combination of silicon dioxide, micronized wax and aluminum oxide.
[0014] As a preferred embodiment, the weight ratio of silicon dioxide, micropowder wax and aluminum oxide is (1-10): (1-10): (1-10).
[0015] As a preferred embodiment, the weight ratio of silicon dioxide, micropowder wax and aluminum oxide is (5-10): (1-5): (1-5).
[0016] As a preferred embodiment, the weight ratio of silicon dioxide, micropowder wax and aluminum oxide is 5:3:3.
[0017] As a preferred embodiment, the viscosity of the copolymerized amine acrylic resin at 25° C. is 1000-1500s.
[0018] As a preferred embodiment, the viscosity of the copolymerized amine acrylic resin at 25° C. is 1200 s.
[0019] As a preferred embodiment, the structure of the dispersant is a modified polyacrylate polymer, and the amine value of the modified polyacrylate polymer is 23-28 mgKOH / g.
[0020] As a preferred embodiment, the amine value of the modified polyacrylate polymer is 25 mgKOH / g.
[0021] As a preferred embodiment, the polyester acrylate is a hyperbranched polyester acrylate with a functionality of 6-8, and the viscosity of the polyester acrylate at 25° C. is 1200-2000 cps.
[0022] As a preferred embodiment, the polyester acrylate is a hyperbranched polyester acrylate with a functionality of 8, and the viscosity of the polyester acrylate at 25° C. is 1200-2000 cps.
[0023] As a preferred embodiment, the chromaticity of the polyester acrylate is ≤1, and the density of the polyester acrylate at 25°C is 1-1.2 g / cm 3 The acid value of the polyester acrylate is ≤2 mgKOH / g, and the refractive index is 1.4-1.5.
[0024] As a preferred embodiment, the chromaticity of the polyester acrylate is ≤1, and the density of the polyester acrylate at 25°C is 1.1 g / cm 3 The acid value of the polyester acrylate is ≤2 mgKOH / g, and the refractive index is 1.485.
[0025] As a preferred embodiment, the epoxy acrylate is a low-viscosity epoxy acrylate with a functionality of 2-6, and the viscosity of the epoxy acrylate is 800-1500 cps.
[0026] As a preferred embodiment, the epoxy acrylate is a low-viscosity epoxy acrylate with a functionality of 4, and the viscosity of the epoxy acrylate is 800-1500 cps.
[0027] As a preferred embodiment, the modified acrylate is a combination of epoxy acrylate and polyester acrylate.
[0028] As a preferred embodiment, the weight ratio of the epoxy acrylate to the polyester acrylate is (5-15):(10-30).
[0029] As a preferred embodiment, the weight ratio of the epoxy acrylate to the polyester acrylate is (5-10):(15-20).
[0030] As a preferred embodiment, the weight ratio of the epoxy acrylate to the polyester acrylate is 8:18.
[0031] As a preferred embodiment, the initiator is a photoinitiator, and the photoinitiator includes a combination of ITX and 1173. Preferably, the weight ratio of ITX to 1173 is (1-5): (2-5).
[0032] As a preferred embodiment, the weight ratio of ITX to 1173 is (1-2): (4-5).
[0033] As a preferred embodiment, the weight ratio of ITX to 1173 is 2:4.
[0034] As a preferred embodiment, the aluminum oxide is gas phase nano aluminum oxide, and the particle size of the aluminum oxide is 30-50 nm.
[0035] During the experiment, the applicant found that by using a monomer combination of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate, and controlling the mass of the monomers to be less than 70%, a UV-curing coating with matching viscosity and surface tension can be obtained, achieving good construction and coating effects. The possible reason is guessed to be: the combination of five monomers of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate can achieve a scientific match between viscosity and surface tension, so that the cured coating can be easily attached to the surface of the substrate and achieve good gloss. The applicant further found that if the monomer content exceeds 70%, the coating will have sedimentation problems, resulting in inconsistent color of the coating appearance and easy stratification after construction.
[0036] The applicant further discovered that by introducing a combination of silica, micronized wax and alumina, the gloss and scratch resistance of the coating can be further improved. The reason may be that the combination of silica, micronized wax and alumina can increase the hardness of the coating and increase the wear resistance of the coating. The applicant also unexpectedly discovered that the surface of the formed coating feels smooth and can achieve good iodine stain resistance.
[0037] A second aspect of the present invention provides a method for preparing a crack-resistant and high-adhesion UV-curable coating, comprising the following steps:
[0038] S1: Stir the monomer combination, copolymerization amine acrylic resin, mixed high molecular polymer, acrylic copolymer solution and dispersant in a high-speed disperser for 10-60 minutes at a speed of 1000-2000 r / min;
[0039] S2 adds initiator and stirs for 30-100min at a speed of 1000-2000r / min;
[0040] Add modified acrylate to S3 and stir for 10-60 minutes at a speed of 1000-2000 r / min;
[0041] Add solid filler to S4, stir for 30-60 minutes at a speed of 1000-3000r / min to obtain.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The crack-resistant and high-adhesion UV-curing coating of the present invention uses a monomer combination of less than 70 parts by weight to obtain a UV-curing coating with matching viscosity and surface tension, achieving good construction and coating effects.
[0044] (2) The crack-resistant and high-adhesion UV-curing coating of the present invention uses a variety of acrylic resin polymer additives to optimize the final coating effect of the coating. The coating is mechanized for construction, overcoming the human factors in manual operation, and the product has a small color difference and stable quality.
[0045] (3) The crack-resistant and high-adhesion UV-curable coating of the present invention can further improve the gloss and scratch resistance of the coating by introducing a combination of silicon dioxide, micro-powder wax and aluminum oxide, and is environmentally friendly and construction-friendly.
[0046] (4) The crack-resistant and high-adhesion UV-curable coating of the present invention can be applied to a substrate made of bamboo or wood to achieve wear resistance of the coating and a smooth surface touch. During the coating process, the coating can decompose harmful substances in the board and can be cured and dried by ultraviolet light, making the product healthier and more environmentally friendly.
[0047] (5) The crack-resistant and high-adhesion UV-curing coating of the present invention is a truly green and environmentally friendly paint that does not contain volatile substances. The products produced on the UV coating production line are green, healthy and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The actual effect picture of the product after painting with the paint of the market competitor;
[0049] Figure 2 This is a real effect diagram after the paint of Example 3 of the present invention is applied;
[0050] Figure 3 The friction effect diagram of the paint of the market competitor after brushing;
[0051] Figure 4 This is a diagram showing the friction effect of the paint of Example 3 of the present invention after being applied. DETAILED DESCRIPTION
[0052] Example
[0053] A crack-resistant and high-adhesion UV-curable coating, the raw materials for preparation are shown in Table 1 below in parts by weight:
[0054] Table 1
[0055]
[0056]
[0057] The copolymerized amine acrylic resin is EBECRYL 7100; the mixed high molecular polymer is TEGODispers 685; the acrylic copolymer solution is BYK ANTI-TERRA-210; the chemical structure of the dispersant is a modified polyacrylate polymer, the amine value of the modified polyacrylate polymer is 25 mgKOH / g, and it is purchased from BASF DispexUltra PA4560.
[0058] The epoxy acrylate is a low-viscosity epoxy acrylate with a functionality of 4 and a viscosity of 800-1500 cps, purchased from Lancolu L-6113.
[0059] The polyester acrylate is a hyperbranched polyester acrylate with a functionality of 8, the viscosity of the polyester acrylate at 25° C. is 1200-2000 cps, the chromaticity of the polyester acrylate is ≤1, and the density of the polyester acrylate at 25° C. is 1.1 g / cm 3 The polyester acrylate has an acid value of ≤2 mgKOH / g and a refractive index of 1.485, and is purchased from Lancolu L-6127.
[0060] The silicon dioxide is from Sigma-Aldrich, the micro powder wax is Tianshi Twax-1045, and the alumina is fumed nano alumina with a particle size of 30-50 nm purchased from Yingcheng YC-QL30.
[0061] A method for preparing a crack-resistant and high-adhesion UV-curing coating comprises the following steps:
[0062] S1: Mix the monomers, copolymerize the amine acrylic resin, mix the high molecular weight polymer, the acrylic copolymer solution, and the dispersant in a high-speed disperser and stir for 30 minutes at a speed of 1500 r / min;
[0063] Add initiator to S2 and stir for 65 min at a speed of 1500 r / min;
[0064] Add modified acrylate to S3 and stir for 30 min at a speed of 1500 r / min;
[0065] Add solid filler to S4 and stir for 45 minutes at a speed of 2000r / min to obtain the product.
[0066] Performance Testing
[0067] 1. Viscosity test: Use a rotational viscometer to test the viscosity at 25°C. Test each sample 3 times and take the average value.
[0068] 2. Density test: Use a density cup to test the gel time at 25°C. Test each sample 3 times and take the average value.
[0069] 3. Surface tension test: Use a liquid surface tension meter to test the surface tension of the coating at room temperature. Test each sample 3 times and take the average value. When testing the surface tension, use an infrared temperature gun to test and record the actual temperature during the test.
[0070] 4. Fineness test: Use a fineness plate to test the fineness at room temperature. Test each sample 3 times and take the average value.
[0071] 5. Prepare, cure and test the coating:
[0072] 5.1.1 Preparation of coating: preheat the coating and bamboo-wood composite baseboard to 45°C, and use a coating film forming device (10-100 μm) to evenly cover the coating on the base material, ensuring that the coating temperature is around 40°C;
[0073] 5.1.2 Curing coating: Place the coating sample under a UV lamp (500-1500mJ / cm 2 ) and allowed to stand for 30 minutes, and then the performance of the cured coating was tested. Figure 1-2 .
[0074] 5.2 Paint hiding power test: Use a colorimeter to test the color difference before and after the paint is applied. For each sample, test ten points and take the average value.
[0075] 5.3 Paint gloss test: Use a gloss meter to test the gloss of the cured coating. For each sample, test ten points and take the average value.
[0076] 5.4 Paint stain resistance test: Use a colorimeter, apply iodine tincture for 1 minute and then wipe it off, and compare the increase in the b value before and after. Test each sample 3 times and take the average value.
[0077] 5.5 Friction test: Use double-sided tape to stick the cut 200-grit sandpaper to the bottom of the friction weight, and push and pull it back and forth horizontally on one side of the ruler 5 times.
[0078] The test results are shown in Table 2.
[0079] Table 2
[0080]
Claims
1. A crack-resistant and high-adhesion UV-curing coating, characterized in that: The raw materials for preparation include, by weight: 115-220 parts of monomer combination, 15-20 parts of copolymerized amine acrylic resin, 0.5-5 parts of mixed high molecular polymer, 0.5-5 parts of acrylic copolymer solution, 0.5-5 parts of dispersant, 10-30 parts of initiator, 50-80 parts of modified acrylate and 35-105 parts of solid filler.
2. The crack-resistant and high-adhesion UV-curing coating according to claim 1, characterized in that: The modified acrylate is selected from one or a combination of epoxy acrylate, polyester acrylate, polyurethane acrylate, and silicone modified acrylate.
3. The crack-resistant and high-adhesion UV-curing coating according to claim 1, characterized in that: The monomer combination is selected from one or a combination of trimethylolpropane triacrylate, tripropylene glycol diacrylate, pentaerythritol triacrylate, 1,6-hexanediol diacrylate, and glycidyl methacrylate.
4. The crack-resistant and high-adhesion UV-curing coating according to claim 1, characterized in that: The solid filler is selected from one or a combination of silicon dioxide, micronized wax, aluminum oxide, talc, and calcium carbonate.
5. The crack-resistant and high-adhesion UV-curing coating according to claim 1, characterized in that: The viscosity of the copolymerized amine acrylic resin at 25° C. is 1000-1500 cps.
6. The crack-resistant and high-adhesion UV-curing coating according to claim 1, characterized in that: The chemical structure of the dispersant is a modified polyacrylate polymer, and the amine value of the modified polyacrylate polymer is 23-28 mgKOH / g.
7. The crack-resistant and high-adhesion UV-curing coating according to claim 2, characterized in that: The polyester acrylate is a hyperbranched polyester acrylate with a functionality of 6-8, and the viscosity of the polyester acrylate at 25° C. is 1200-2000 cps.
8. The crack-resistant and high-adhesion UV-curing coating according to claim 2, characterized in that: The epoxy acrylate is a low-viscosity epoxy acrylate with a functionality of 2-6, and the viscosity of the epoxy acrylate is 800-1500 cps.
9. The crack-resistant and high-adhesion UV-curing coating according to claim 4, characterized in that: The aluminum oxide is gas phase nano aluminum oxide, and the particle size of the aluminum oxide is 30-50 nm.
10. A method for preparing the crack-resistant and high-adhesion UV-curable coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1: Stir the monomer combination, copolymerization amine acrylic resin, mixed high molecular polymer, acrylic copolymer solution and dispersant in a high-speed disperser for 10-60 minutes at a speed of 1000-2000 r / min; Add initiator to S2 and stir for 30-100 min at a speed of 1000-2000 r / min; Add modified acrylate to S3 and stir for 10-60 minutes at a speed of 1000-2000 r / min; Add solid filler to S4, stir for 30-60 minutes at a speed of 1000-3000r / min to obtain.
Citation Information
Patent Citations
UV curing color decorative coating
CN101407651A
UV-cured protective coating and preparation method thereof
CN105670490A
High-toughness epoxy powder coating
CN109651932A
Novel water-based ultraviolet-curing wear-resistant coating as well as preparation method and use method thereof
CN112480805A
Ultraviolet photocureable coating applied to powder spraying
CN115651501A