Pneumatic-scouring-resistant low-absorption low-emission thermal control coating, coating as well as preparation method and application of coating
Through the multi-layer coating structure design, combined with the characteristics of the bottom, middle and surface layer, the problem of poor stability of the existing thermal control coating in high temperature and high speed environments is solved, and the long-term insulation and thermal insulation of spacecraft in multiple environments is achieved. and protective effect.
Patent Information
- Application Number
- CN202411107274.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing low absorption and low emission thermal control coating cannot remain stable under high temperature and high-speed airflow erosion environments, and cannot meet the thermal insulation functions of large-sized return spacecraft in various harsh environments.
Using a multi-layer coating structure design, including the bottom layer, middle layer and surface layer. The bottom layer is a high-temperature resistant coating. The middle layer has thermal conductivity and heat resistance. The surface layer plays a thermal radiation inhibitory role in a high vacuum environment to ensure that the spacecraft is complex. Long-term stability in the environment.
It realizes thermal insulation and insulation of spacecraft in high-temperature and high-speed airflow erosion environments, extends the service life of the coating, and provides rain protection and thermal insulation protection in rocket launch towers and launch ascending sections, improving the multi-environment of spacecraft Adaptability.
Smart Images

Figure CN119060628A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of surface engineering technology, and particularly relates to an aerodynamic erosion-resistant, low-absorption, low-emission thermal control paint, coating, and preparation method and application thereof, which are adaptable to various harsh environmental conditions such as the rocket launch waiting stage, launch ascent stage and space flight stage of large-sized recoverable spacecraft without rocket fairing protection. Background Art
[0002] Thermal control coating is an important component of the thermal control system of spacecraft, and plays an important role in the thermal balance of spacecraft in the high vacuum space environment. At present, the outer surface of my country's spacecraft uses low-absorption and low-emission thermal control coatings, which have the function of reducing solar radiation absorption and infrared radiation heat dissipation. It can play a certain role in heat preservation for the complex temperature environment experienced by spacecraft in solar radiation and deep cold space, and improve the comfort level in the cabin.
[0003] As the size and weight of spacecraft continue to increase, the transportation space and power of rockets are limited. Therefore, in the future, large-sized returning spacecraft may no longer be protected by rocket fairings, resulting in the cabin directly facing the rainfall environment of the rocket launch tower and the high temperature and high-speed airflow scouring environment of the rocket launch ascent phase. This requires that the thermal control coating, in addition to the original properties of resistance to alternating high and low temperatures and space radiation, also needs to have new properties such as resistance to rain and resistance to high-temperature and high-speed aerodynamic scouring.
[0004] The low-absorption and low-emission thermal control coatings of existing spacecraft are silicone resin system thermal control coatings, which have certain hydrophobic properties and can play a certain role in rain protection. However, the heat resistance limit of silicone resin is 300-400℃. Excessive temperature will cause the resin to cyclize, crack and fall off. Therefore, in the high temperature and high-speed airflow environment of 500-600℃ in the rocket's ascent stage, the existing low-absorption and low-emission thermal control coatings will be thermally decomposed and fall off, and cannot meet the thermal insulation function in the subsequent space environment. At the same time, in order to ensure that the anti-thermal ablation materials used in large-sized returning spacecraft are not thermally decomposed in advance in the rocket's ascent stage, the outermost wall thermal control coating needs to have certain aerodynamic environment thermal insulation properties to reduce the heat transferred from aerodynamic heat to the anti-thermal ablation materials. The thermal control coatings in the prior art cannot meet the above requirements at the same time. In order to improve the operating stability of large returning spacecraft in multiple environments, it is of great research significance and application background to provide a low-absorption and low-emission thermal control coating resistant to aerodynamic thermal environment and its preparation method. Summary of the invention
[0005] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided an aerodynamic erosion-resistant, low-absorption, low-emission thermal control coating, coating, and preparation method and application thereof. The thermal control coating includes a bottom layer, a middle layer and a surface layer. The surface layer inhibits thermal radiation in a high vacuum environment in space and ensures stability in a long-term space radiation environment, thereby playing a long-term thermal insulation function for the interior of a large-sized recoverable spacecraft. The middle layer is used to enhance the bonding force between the surface layer and the bottom layer. At the same time, the middle layer itself has certain heat resistance and thermal conductivity under aerodynamic environments to prevent heat from staying in the surface layer and causing thermal damage to the surface layer. The bottom layer is a high-temperature resistant coating and provides excellent thermal insulation performance between the coating and the substrate (anti-thermal ablation layer) under aerodynamic environments to avoid the substrate (ablation anti-thermal layer) of the recoverable spacecraft from being heated and burned under the aerodynamic thermal environment of the rocket's ascent phase.
[0006] The technical solution provided by the present invention is as follows:
[0007] In a first aspect, a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion comprises a base coating, a middle coating and a surface coating;
[0008] (I) The primer includes the following raw materials in parts by weight:
[0009] Component unit A:
[0010]
[0011] Component unit B includes ethylene glycol and hollow glass microspheres. The amount of hollow glass microspheres added to solution B is 25-30% of the volume of component unit A, and the amount of ethylene glycol added is 25-30% of the volume of component unit A.
[0012] (II) The middle layer coating comprises the following raw materials in parts by weight:
[0013] Component unit A:
[0014]
[0015] Component unit B:
[0016] Curing agent I 4-10 parts;
[0017] (III) The surface coating comprises the following raw materials in parts by weight:
[0018] Component unit A:
[0019]
[0020] Component unit B:
[0021] 1 to 3 parts of curing catalyst;
[0022] Curing agent II 4 to 7 parts.
[0023] In a second aspect, a method for preparing a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion comprises:
[0024] A silicate aqueous solution, deionized water, silica sol, silane coupling agent and powder are mixed and ball-milled to form component unit A; ethylene glycol is added to the hollow glass microspheres to uniformly wet the hollow glass microspheres to obtain component unit B; component unit B is mixed and stirred with component unit A to obtain a uniformly dispersed base coating;
[0025] The methylphenyl silicone resin and the solvent are mixed evenly, fillers and glass beads are added, sand milled and stirred, and curing agent I is added before preparing the coating to obtain a uniformly dispersed middle layer coating;
[0026] Add solvent, flaky aluminum powder and silane coupling agent to the silicone resin, mix and stir to evenly disperse the filler, add curing agent II and curing catalyst before preparing the coating to obtain an evenly dispersed surface coating.
[0027] In a third aspect, an aerodynamic erosion resistant low-absorption low-emission thermal control coating is prepared using the aerodynamic erosion resistant low-absorption low-emission thermal control coating described in the first aspect to form a composite coating of a bottom layer, a middle layer and a surface layer.
[0028] In the fourth aspect, a method for preparing a low-absorption, low-emission thermal control coating resistant to aerodynamic erosion is provided, comprising: spraying a base coating on the surface of a substrate, spraying a middle coating after the base coating is cured, spraying a top coating after the middle coating is cured, and baking and curing to obtain a low-absorption, low-emission thermal control coating resistant to aerodynamic erosion.
[0029] The fifth aspect is the application of an aerodynamic erosion-resistant, low-absorption, low-emission thermal control coating as a thermal control coating for the in-orbit segment of a spacecraft, or as a rainproof and anti-corrosion coating on the surface of a spacecraft cabin in the absence of a rocket fairing during the launch waiting phase, or as an aerodynamic erosion-resistant coating on the surface of a spacecraft cabin in the absence of a rocket fairing during the rocket launch ascent phase.
[0030] According to the present invention, a low-absorption, low-emission thermal control coating, coating and preparation method and application thereof that are resistant to aerodynamic erosion have the following beneficial effects:
[0031] (1) The present invention provides an aerodynamic erosion-resistant low-absorption and low-emission thermal control coating, coating, and preparation method and application thereof. A new thermal control coating with bottom layer heat insulation, middle layer heat conduction and heat resistance, and surface layer stable low absorption and low emission performance is formed through composite multi-layer functional coating structure design and interface matching design inside the coating; the bottom layer is a high-temperature resistant coating, and provides excellent thermal insulation performance between the coating and the substrate (thermal ablation layer) to prevent the substrate (ablation heat protection layer) of the returning spacecraft from being heated and burned in the aerodynamic thermal environment of the rocket's ascent stage;
[0032] (2) The present invention provides a kind of aerodynamic erosion resistant low absorption and low emission thermal control coating, coating and its preparation method and application, which plays a role in sealing the bottom inorganic thermal control coating, controlling the interface bonding force, buffering and matching the interface mechanics, and ensuring multiple waterproof application performances through the transition of the middle layer that is resistant to high temperature and heat conductive. It meets the requirements of high temperature resistance, heat insulation and waterproofness of the coating while ensuring the thermal control requirements of the surface application and the long-term space environment stability requirements;
[0033] (3) The present invention provides an aerodynamic erosion-resistant low-absorption and low-emission thermal control paint, coating, and preparation method and application thereof. The surface layer can inhibit thermal radiation in a high vacuum environment in space and ensure stability in a space environment, thereby providing long-term thermal insulation for the interior of a returning spacecraft.
[0034] (4) The present invention provides an aerodynamic erosion-resistant, low-absorption, low-emission thermal control coating, coating, and preparation method and application thereof. The thermal control coating is no longer limited to the thermal control effect on the surface of the spacecraft in orbit in the space segment like traditional thermal control coatings or coating materials. It also adds the function of protecting the spacecraft cabin without the protection of the rocket fairing on the rocket launch tower from rain, and the function of thermal insulation protection for the spacecraft cabin without the protection of the rocket fairing in the rocket launch ascent segment. That is, under the preparation method, the thermal control coating is extended from playing a role only in the space segment to playing a role in the launch waiting segment and the launch segment;
[0035] (5) The present invention provides a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion, which has the following characteristics:
[0036] (a) Appearance: metallic color, uniform surface, no blistering, no cracking, no shedding;
[0037] (b) Thickness: 160-290 μm (bottom layer thickness is 100-200 μm, middle layer thickness is 20-40 μm, and surface layer thickness is 40-50 μm);
[0038] (c) Solar absorption ratio: 0.15±0.02;
[0039] (d) Hemispheric emissivity: 0.16±0.02.
[0040] (e) Thermal cycle performance: After 100 cycles of normal pressure thermal cycle tests at -196℃~150℃, the appearance color is uniform, there is no obvious color difference, the coating does not fall off, and the thermal radiation performance (solar absorption ratio and hemispherical emissivity) does not change;
[0041] (f) Aerodynamic thermal resistance: The coating has no appearance change after 180 to 240 seconds of high-temperature, high-speed aerodynamic scouring (airflow recovery enthalpy 730KJ / kg, shear force 114Pa, time not less than 60s, airflow recovery enthalpy 1247KJ / kg, shear force 29Pa, time not less than 30s). The maximum temperature resistance of the low-absorption, low-emission thermal control coating can be stably maintained in an aerobic environment of 580°C for 180 seconds.
[0042] (g) Thermal insulation performance: The thermal conductivity of the coating is in the range of 0.13 to 0.16 W / m·k at room temperature. Within this range, when the coating is washed by high-temperature and high-speed airflow, the heat will not stay in the organic middle layer and surface layer for a long time after accumulation, but will transfer the heat to the bottom layer. Moreover, under this thermal conductivity, the bottom, middle and surface layers have a certain thermal insulation capacity, which can prevent the coating from being heated and burned within 180 to 240 seconds in the ascending section.
[0043] (h) Waterproof performance: The water absorption rate of the coating after being exposed to rain for 24 hours is less than 0.5%;
[0044] (i) The coating adhesion is better than Grade 1 using the cross-cut test. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a structural diagram of a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion according to the present invention;
[0046] Figure 2 This is an appearance diagram of a low-absorption, low-emission thermal control coating structure resistant to aerodynamic erosion in Example 1, wherein (a) is an appearance diagram of the coating on a heat-resistant material; (b) is an appearance diagram of the coating after undergoing a normal pressure thermal cycle;
[0047] Figure 3 This is an appearance diagram of a low-absorption and low-emission thermal control coating junction resistant to aerodynamic erosion after a thermal erosion test in Example 1;
[0048] Figure 4 This is the appearance of the coating in Comparative Examples 1-8 after the air heat scouring test;
[0049] Figure 5 The temperature data monitoring curve of the heat-resistant cabin body using the low-absorption and low-emission thermal control coating resistant to aerodynamic thermal environment of Example 1 during in-orbit flight in space is shown in that the cabin wall temperature is within the range of 7 to 16° C. after being stabilized in orbit, and the temperature control performance is good;
[0050] Figure 6 This is a temperature data monitoring curve of a heat-resistant cabin using the aerodynamic thermal environment resistant low-absorption and low-emission thermal control coating of Example 1 during in-orbit flight in space. After being stabilized in orbit, the air temperature in the cabin is within the range of 10-15°C, and the temperature control performance is good. DETAILED DESCRIPTION
[0051] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0052] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.
[0053] The present invention provides a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion. The formed coating comprises a bottom layer, a middle layer and a surface layer from the surface of the substrate. The thickness of the bottom layer is 100 to 200 μm, the thickness of the middle layer is 20 to 40 μm, and the thickness of the surface layer is 40 to 50 μm. Figure 1 ;
[0054] (I) The primer includes the following raw materials in parts by weight:
[0055] Component unit A:
[0056]
[0057]
[0058] The component unit B includes ethylene glycol and hollow glass microspheres. The amount of the hollow glass microspheres added in the solution B is 25-30% of the volume of the component unit A, and the amount of the ethylene glycol added is 25-30% of the volume of the component unit A.
[0059] The base coating uses silicate and silica sol as binders, zirconium oxide, zinc oxide and / or zinc titanate powder, hollow glass microspheres as fillers, deionized water and ethylene glycol as solvents, and a silane coupling agent is added. The silicate aqueous solution is at least one of potassium silicate aqueous solution or lithium silicate aqueous solution, with a mass concentration of 25-35%; the mass concentration of the silica sol is 20%-40%; the silane coupling agent is at least one of KH550 or KH560; the ethylene glycol is analytically pure; and the particle size of the hollow glass microspheres is 25-90 microns.
[0060] (II) The middle layer coating comprises the following raw materials in parts by weight:
[0061] Component unit A:
[0062]
[0063] Component unit B:
[0064] Curing agent I 4 to 10 parts.
[0065] Curing agent I is a polysilazane crosslinking agent.
[0066] Methylphenyl silicone resin is a hydroxyl-terminated methylphenyl silicone resin.
[0067] The filler is a mixed filler of aluminum oxide, titanium oxide, silicon carbide and mica powder, with 50-90 parts of aluminum oxide, 50-90 parts of titanium oxide, 10-20 parts of silicon carbide and 30-50 parts of mica powder; the silicon carbide filler is beta phase nano silicon carbide with a particle size of 50-500nm.
[0068] The particle size of the glass beads is 2 to 3 mm.
[0069] The solvent is at least one of butyl acetate or xylene.
[0070] (III) The surface coating comprises the following raw materials in parts by weight:
[0071] Component unit A:
[0072] 100 parts of silicone resin;
[0073] 100-150 parts of flake aluminum powder;
[0074] Silane coupling agent 2-5 parts;
[0075] Solvent 70-100 parts
[0076] Component unit B:
[0077] 1 to 3 parts of curing catalyst;
[0078] Curing agent II 4 to 7 parts.
[0079] The organic silicone resin is at least one of polydimethyl silicone resin and polydimethyl silicone rubber.
[0080] The diameter of the flaky aluminum powder is 40 to 60 μm.
[0081] The silane coupling agent is at least one of KH550 and KH560.
[0082] The solvent is at least one of butyl acetate and xylene.
[0083] The curing catalyst is dibutyltin dilaurate.
[0084] Curing agent II is ethyl orthosilicate.
[0085] The present invention also provides a method for preparing aerodynamic erosion resistant low-absorption and low-emission thermal control coating and a method for forming a thermal control coating using the thermal control coating, comprising the following steps:
[0086] Preparation of base coating: deionized water is added to the silicate aqueous solution, mixed and stirred, silica sol and silane coupling agent are slowly added, stirring is continued, powder is added, ball milling is performed to disperse the filler evenly to form component unit A; ethylene glycol is added to the hollow glass microspheres to wet the hollow glass microspheres evenly to obtain component unit B, component unit B is mixed and stirred with component unit A to obtain a uniformly dispersed base coating.
[0087] In this step, the alumina balls used in the ball milling process have a rotation speed of 70 to 120 r / min and a ball milling dispersion time of 10 to 14 h.
[0088] In this step, during the mixing and stirring process of component unit B and component unit A, a stirrer is used for dispersion stirring at a speed of 400 to 500 r / min for 2 to 3 hours.
[0089] Preparation of the middle layer coating: Mix the methylphenyl silicone resin and the solvent evenly, add fillers and glass beads, sand grind and stir, and add curing agent I before preparing the coating to obtain a uniformly dispersed middle layer coating. During the sand grinding and stirring process in this step, the speed of the disperser is 1200-1500 r / min, and the dispersion time is 2-4 hours.
[0090] Preparation of surface coating: Add solvent, flaky aluminum powder and silane coupling agent to silicone resin, mix and stir to disperse the filler evenly, add curing agent II and curing catalyst before preparing the coating to obtain a uniformly dispersed surface coating. During the stirring process of this step, the speed of the disperser is 300-500r / min, and the dispersion time is 2-4h.
[0091] Coating preparation: The coating is prepared by air spraying. First, spray the base coat on the surface of the substrate. After the base coat is cured, spray the middle coat. After the middle coat is cured, spray the top coat. After baking and curing for 12 to 24 hours, a low-absorption, low-emission thermal control coating resistant to aerodynamic erosion is obtained.
[0092] The thickness of the bottom layer spraying is 100-200 μm, and the curing system used is 60-100°C for 12-24 hours, preferably 80°C for 24 hours. The thickness of the middle layer spraying is 20-40 μm, and the curing system used is 80-150°C for 12-24 hours, preferably 150°C for 12 hours. The thickness of the surface layer spraying is 40-50 μm, and the curing system used is 60-100°C for 24 hours, preferably 80°C for 24 hours.
[0093] Example
[0094] Example 1
[0095] A method for preparing aerodynamic erosion-resistant low-absorption and low-emission thermal control coating comprises the following steps:
[0096] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, use a ball mill to disperse, speed 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir with a stirrer, speed 500r / min, stir for 2h, and obtain base coating.
[0097] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenyl silicone resin and 60 g of butyl acetate into a flask, mix well, add 28 g of aluminum oxide powder, 28 g of titanium oxide powder, 5.6 g of beta-phase nano silicon carbide (particle size 50-500 nm), 18.4 g of mica powder, 130 g of glass beads (particle size 2-3 mm), and disperse by sand milling at 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0098] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0099] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0100] The coating prepared in this example: a) has a metallic appearance, a uniform surface, no blistering, no cracks, no peeling, Figure 2a; b) Thickness: 184-203μm (bottom layer 122-133μm + middle layer 21-25μm + surface layer 41-45μm); c) Solar absorption ratio: 0.13; d) Hemispherical emissivity: 0.16; e) Thermal cycle performance: After the -196℃~150℃, 100 times normal pressure thermal cycle test, the coating has uniform appearance color, no obvious color difference, the coating does not fall off, and the thermal physical properties are stable. Figure 2 b; f) Heat resistance: After 180s of high-temperature, high-speed pneumatic flushing, the coating appearance does not change, see Figure 3 ; g) Thermal insulation performance: The thermal conductivity of the coating at room temperature is 0.155W / m·k; h) Waterproof performance: The water absorption rate of the coating after 24 hours in the rain environment is 0.4%; i) The adhesion of the coating is better than level 1 using the cross-cut test. The temperature data monitoring curve of the heat-resistant cabin body using the aerodynamic thermal environment resistant low absorption and low emission thermal control coating of Example 1 during in-orbit flight in space shows that the cabin wall temperature and the cabin air temperature are within the range of 7 to 16°C and 10 to 15°C respectively after being stabilized on orbit, and the temperature control performance is good, see Figure 5 and Figure 6 .
[0101] Example 2
[0102] A method for preparing aerodynamic erosion-resistant low-absorption and low-emission thermal control coating comprises the following steps:
[0103] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 73g zinc oxide powder filler, pour the mixed solution into a ball mill, use a ball mill to disperse at a speed of 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, use a stirrer to disperse and stir at a speed of 500r / min, stir for 2h, and obtain the base coating.
[0104] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenylsiloxane resin and 60 g of butyl acetate into a flask, mix well, add 21 g of alumina powder, 21 g of titanium oxide powder, 4.2 g of beta-phase nano silicon carbide filler (particle size 50-500 nm), 13.8 g of mica powder, 90 g of glass beads (particle size 2-3 mm), and disperse by sand milling at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0105] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0106] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0107] The coating prepared in this example: a) metallic appearance, uniform surface, no blistering, no cracks, no falling off; b) thickness: 185-199μm (bottom layer 123-129μm + middle layer 20-25μm + surface layer 42-45μm); c) solar absorption ratio: 0.13; d) hemispherical emissivity: 0.16; e) thermal cycle performance: after -196℃~150℃, 100 times normal pressure thermal cycle test, the coating has uniform appearance color, no obvious color difference, no coating falling off, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the appearance of the coating has no change; g) thermal insulation performance: the thermal conductivity of the coating is 0.153W / m·k at room temperature; h) waterproof performance: the water absorption rate of the coating is 0.4% after 24h in rain environment; i) the adhesion of the coating is better than level 1 using the cross-cut test.
[0108] Comparative Example
[0109] Comparative Example 1
[0110] The raw material composition, dosage and preparation process used in Comparative Example 1 are basically consistent with those in Example 1, except that the amount of zinc orthotitanate powder as filler added in the primer is different.
[0111] The steps of coating preparation include:
[0112] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.34g silane coupling agent KH560, stir for 1h, add 110g zinc titanate powder filler, pour the mixed solution into a ball mill, disperse using a ball mill, the alumina ball used in the ball milling process rotates at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir using a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0113] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenyl silicone resin and 60 g of butyl acetate into a flask and mix well. Then add 28 g of alumina powder, 28 g of titanium oxide powder, 5.6 g of beta-phase nano silicon carbide filler (particle size 50-500 nm), 18.4 g of mica powder, and 130 g of glass beads (particle size 2-3 mm). Then, grind and disperse at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0114] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0115] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0116] The coating prepared in this comparative example has a large amount of powder filler added to the bottom layer, which causes the coating to crack. Cracks are still visible after the middle layer and the surface layer are sprayed. The appearance is metallic color, the surface is uniform, and there is no blistering or cracking. However, after the cross-cut test of the bonding strength, the coating bonding strength is poor. After the high temperature and high speed pneumatic scouring test, the surface layer peels and the bottom layer falls off from the substrate, which cannot meet the subsequent use and performance test requirements. Figure 4 .
[0117] Comparative Example 2
[0118] The raw material composition, dosage and preparation process used in Comparative Example 2 are basically consistent with those in Example 1, except that the amount of hollow glass microspheres added in the base coating is higher.
[0119] The steps of coating preparation include:
[0120] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.21g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, disperse using a ball mill, the alumina ball used in the ball milling process rotates at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 35% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir using a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0121] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenylsiloxane resin and 60 g of butyl acetate into a flask, mix well, add 28 g of aluminum oxide powder, 28 g of titanium oxide powder, 5.6 g of beta-phase nano silicon carbide (particle size 50-500 nm), 18.4 g of mica powder, 130 g of glass beads (particle size 2-3 mm), and disperse by sand milling at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0122] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0123] (3) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0124] The coating prepared in this comparative example: a) metallic color, uniform surface, no blistering, no cracks, no shedding; b) thickness: 190-202μm (bottom layer 128-132μm + middle layer 21-25μm + surface layer 41-45μm); c) solar absorption ratio: 0.15; d) hemispherical emissivity: 0.16; e) thermal cycle performance: after 100 times of normal pressure thermal cycle test at -196℃~150℃, the coating has uniform color, no obvious color difference, no shedding, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating cracks and peels, and the coating is Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.123W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.4% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0125] The amount of hollow glass microspheres added to the bottom layer increases, and the thermal conductivity of the coating decreases, which improves the thermal insulation performance of the bottom layer and the overall coating. However, after the thermal insulation performance of the bottom layer is improved, the heat transmitted from the outside cannot continue to be conducted downward after reaching the inorganic bottom layer, which eventually causes a large amount of heat to accumulate in the bottom layer, thereby increasing the overall temperature of the composite coating. Therefore, the heat absorbed by the organic middle layer (transition layer) and the organic surface layer also increases significantly, but the heat resistance of the surface layer of the organic thermal control coating is usually around 400°C, so the surface layer after high-temperature and high-speed aerodynamic scouring tests is heated to crack and peel, so the thermal insulation performance of the coating needs to be controlled within a certain range.
[0126] Comparative Example 3
[0127] The raw material composition, dosage and preparation process used in Comparative Example 3 are basically consistent with those in Example 1, except that the amount of hollow glass microspheres added in the bottom layer is lower.
[0128] The steps of coating preparation include:
[0129] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.21g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, disperse using a ball mill, the alumina ball used in the ball milling process rotates at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 5% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir using a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0130] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenyl silicone resin and 60 g of butyl acetate into a flask and mix well. Add 28 g of alumina powder, 28 g of titanium oxide powder, 5.6 g of beta-phase nano silicon carbide filler (particle size 50-500 nm), 18.4 g of mica powder, and 130 g of glass beads (particle size 2-3 mm). Disperse by sand milling at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, free of precipitation, and does not contain a curing agent.
[0131] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0132] (3) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 0.5g of dibutyltin silicate and 2g of polysilazane crosslinking agent to the middle layer coating. Spray the middle layer coating twice. After drying for 24 hours, bake at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin silicate and 2g of ethyl orthosilicate to the top layer coating. Spray the top layer coating 4 times. Dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0133] The coating prepared in this comparative example: a) metallic color, uniform surface, no blistering, no cracks, no shedding; b) thickness: 179-199 μm (bottom layer 110-123 μm + middle layer 25-30 μm + surface layer 44-46 μm); c) solar absorption ratio: 0.15; d) hemispherical emissivity: 0.16; e) thermal cycle performance: after 100 times of normal pressure thermal cycle test at -196℃~150℃, the coating has uniform color, no obvious color difference, no shedding, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating cracks and sees Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.171W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.4% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0134] The amount of hollow glass microspheres added to the bottom layer is reduced, and the thermal conductivity of the coating is increased, which reduces the thermal insulation performance of the bottom layer and the overall coating. After the coating is heated by an external heat source, a large amount of heat is quickly transferred to the heat-resistant material substrate. After continuous accumulation, the heat-resistant material eventually reaches the decomposition temperature and decomposes, which reduces the adhesion stability between the coating and the substrate interface. After experiencing a high temperature environment, the coating will expand and shrink to a certain extent. Therefore, the reduced bonding force between the coating and the substrate interface will cause the coating to crack after being heated. The bottom layer needs to have a certain degree of thermal insulation ability to keep the temperature of the heat-resistant material lower than its decomposition temperature to ensure the stability of the coating.
[0135] Comparative Example 4
[0136] The raw material composition, dosage and preparation process used in Comparative Example 4 are basically consistent with those in Example 1, except that: there is no middle layer in the composite coating.
[0137] The steps of coating preparation include:
[0138] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, disperse using a ball mill, the alumina ball used in the ball milling process rotates at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir using a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0139] (2) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0140] (3) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the surface layer. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the surface layer, spray the surface layer 4 times, dry the coating in the shade at room temperature for 16 hours, and cure it at 80°C for 24 hours to obtain the coating.
[0141] The coating prepared in this comparative example has a metallic appearance, a uniform surface, no bubbles, and no cracks. However, due to the absence of an intermediate layer, the surface layer of the coating system has no bonding force on the bottom layer of the inorganic system. The surface coating containing aluminum powder and silicone resin has poor wettability on the surface of the inorganic coating. After coating, the resin and the filler are separated. After 180s of high-temperature, high-speed pneumatic scouring, the surface layer falls off in pieces, which cannot meet the subsequent thermal control use and performance test requirements. Figure 4 The middle layer, as a transition layer, has a dense organic cross-linking degree and no pores, which can realize the flat arrangement of aluminum powder filler.
[0142] Comparative Example 5
[0143] The raw material composition, dosage and preparation process used in Comparative Example 5 are basically consistent with those in Example 1, except that: there is no surface layer in the composite coating.
[0144] The steps of coating preparation include:
[0145] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, use a ball mill to disperse, use alumina balls in the ball milling process, rotate at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir with a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0146] (2) Preparation of middle layer coating: Add 40g of hydroxyl-terminated methylphenylsiloxane resin and 60g of butyl acetate into a flask, mix well, add 28g of alumina powder, 28g of titanium oxide powder, 5.6g of beta-phase nano silicon carbide filler (particle size 50-500nm), 18.4g of mica powder, 130g of glass beads (particle size 2-3mm), and disperse by sand grinding at a speed of 1400r / min for 2h to obtain a middle layer coating with uniform dispersion, no precipitation, and no curing agent.
[0147] (3) Coating preparation: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 0.5g of dibutyltin disilicate and 2g of polysilazane crosslinking agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours to obtain the coating.
[0148] The coating prepared in this comparative example: a) gray appearance, uniform surface, no blistering, no cracks, no shedding; b) thickness: 140-160 μm; c) solar absorption ratio: 0.60; d) hemispherical emissivity: 0.75; e) thermal cycle performance: after 100 times of normal pressure thermal cycle test at -196℃~150℃, the coating has uniform appearance color, no obvious color difference, no shedding of the coating, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating has no obvious change, see Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.153W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.6% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0149] There is no surface layer in this comparative example, so the thermal radiation performance of the coating cannot be guaranteed. At the same time, since the surface layer is an organic system coating, the organic coating usually has hydrophobic properties, which is conducive to reducing the water absorption rate of the coating. Therefore, the thermal radiation performance and water absorption rate of this comparative example cannot meet the requirements.
[0150] Comparative Example 6
[0151] The raw material composition, dosage and preparation process used in Comparative Example 6 are basically consistent with those in Example 1, except that: the type and amount of filler added in the middle layer coating are different, and no nano-silicon carbide is added.
[0152] The steps of coating preparation include:
[0153] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, use a ball mill to disperse, use alumina balls in the ball milling process, rotate at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir with a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0154] (2) Preparation of middle layer coating: Add 40 g of hydroxyl-terminated methylphenyl silicone resin and 60 g of butyl acetate into a flask and mix well. Add 29 g of aluminum oxide powder, 29 g of titanium oxide powder, 22 g of mica powder and 130 g of glass beads (particle size 2-3 mm). Disperse by sand milling at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, free of precipitation and does not contain a curing agent.
[0155] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0156] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0157] The coating prepared in this comparative example a) has a metallic appearance, a uniform surface, no blistering, no cracks, and no shedding; b) thickness: 182-199 μm (bottom layer 120-125 μm + middle layer 21-25 μm + surface layer 41-49 μm); c) solar absorption ratio: 0.15; d) hemispherical emissivity: 0.17; e) thermal cycle performance: after the coating has been subjected to -196°C to 150°C and 100 times of normal pressure thermal cycle tests, the appearance color of the coating is uniform, there is no obvious color difference, the coating does not fall off, and the thermal physical properties are stable; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating cracks and peels, and the coating is visible Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.125W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.4% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0158] In this example, nano silicon carbide fillers are not added to the middle layer, and silicon carbide materials have a high thermal conductivity, which is conducive to quickly transferring the heat applied by the external heat source of the coating from the surface layer with poor high temperature tolerance to the bottom layer that can withstand high temperatures, effectively ensuring that the surface layer does not accumulate heat, and has a relatively high specific heat capacity in a high temperature environment, that is, after absorbing heat, the temperature rises at a low degree and slow speed, further reducing the temperature that the surface layer needs to withstand in a short period of time. Therefore, not adding nano silicon carbide will cause the surface layer to quickly reach the decomposition temperature of the organic coating system in a high temperature environment, resulting in cracking and peeling.
[0159] Comparative Example 7
[0160] The raw material composition, dosage and preparation process used in Comparative Example 7 are basically the same as those in Example 1, except that the amount of silica sol added in the base coating is increased.
[0161] The steps of coating preparation include:
[0162] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 8g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, disperse using a ball mill, the alumina ball used in the ball milling process rotates at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir using a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0163] (2) Preparation of middle layer coating: Add 40g of hydroxyl-terminated methylphenyl silicone resin and 60g of butyl acetate into a flask, mix well, add 28g of aluminum oxide powder, 28g of titanium oxide powder, 5.6g of beta-phase nano silicon carbide (particle size 50-500nm), 18.4g of mica powder, 130g of glass beads (particle size 2-3mm), and disperse by sand milling at a speed of 1400r / min for 2h to obtain a middle layer coating with uniform dispersion, no precipitation, and no curing agent.
[0164] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0165] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of polysilazane crosslinking agent and curing agent to the middle layer coating, spray the middle layer coating twice, dry for 24 hours, and then cure at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin disilicate and 2g of ethyl orthosilicate to the top layer coating, spray the top layer coating 4 times, dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0166] The coating prepared in this comparative example: a) metallic appearance, uniform surface, no blistering, no cracks, no falling off; b) thickness: 190-200 μm (bottom layer 128-132 μm + middle layer 21-24 μm + surface layer 41-44 μm); c) solar absorption ratio: 0.17; d) hemispherical emissivity: 0.17; e) thermal cycle performance: after -196℃~150℃, 100 times normal pressure thermal cycle test, the coating has uniform appearance color, no obvious color difference, no falling off, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating cracks and peels, and the coating is Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.155W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.3% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0167] The increase in the amount of silica sol added to the base layer improves the density of the coating, which is beneficial to reducing the water absorption rate of the coating. However, the improvement in the density of the base layer affects the interlayer bonding strength of the coating. After high-temperature and high-speed pneumatic scouring, the surface layer is heated and cracked and peeled.
[0168] Comparative Example 8
[0169] The raw material composition, dosage and preparation process used in Comparative Example 8 are basically consistent with those in Example 1, except that: in the selection of the curing agent for the middle layer coating, ethyl orthosilicate and 0.5 g of dibutyltin dilaurate curing agent are selected.
[0170] The steps of coating preparation include:
[0171] (1) Preparation of base coating: Add 60g potassium silicate aqueous solution (concentration 30wt%) and 120g deionized water into a beaker, mix well, add 3g silica sol (concentration 30wt%) during stirring, add 2.15g silane coupling agent KH560, stir for 1h, add 100g zinc titanate powder filler, pour the mixed solution into a ball mill, use a ball mill to disperse, use alumina balls in the ball milling process, rotate at 100r / min, disperse for 12h, and the obtained component unit A is dispersed evenly without precipitation. Add 25% of the volume of component unit A hollow glass microspheres (particle size 25-90μm) into a beaker, wet with the same volume of ethylene glycol, mix with component unit A, disperse and stir with a stirrer at a rotation speed of 500r / min, stir for 2h, and obtain base coating.
[0172] (2) Preparation of middle layer coating: Add 40 g of methylphenyl silicone resin and 60 g of butyl acetate into a flask, mix well, add 28 g of aluminum oxide powder, 28 g of titanium oxide powder, 5.6 g of beta-phase nano silicon carbide (particle size 50-500 nm), 18.4 g of mica powder, 130 g of glass beads (particle size 2-3 mm), and disperse by sand milling at a speed of 1400 r / min for 2 h to obtain a middle layer coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0173] (3) Preparation of surface coating: Add 60g of polydimethylsilicone resin and 45g of butyl acetate into a beaker and mix well. Add 60g of flaky aluminum powder (diameter 40-60μm) and 1.2g of KH560 silane coupling agent. Disperse at a speed of 400r / min for 3h to obtain a surface coating that is evenly dispersed, has no precipitation, and does not contain a curing agent.
[0174] (4) Preparation of coating: First, spray the base layer on the surface of the low-density heat-resistant material. The base layer is sprayed 5 times, dried for 16 hours, and then cured at 80°C for 24 hours. After the base layer is cured, spray the middle layer. Add 2g of ethyl orthosilicate and 0.5g of dibutyltin dilaurate as curing agent to the middle layer coating. Spray the middle layer coating twice. After drying for 24 hours, bake at 150°C for 12 hours. After the middle layer is cured, spray the top layer coating. Add 0.5g of dibutyltin dilaurate and 2g of ethyl orthosilicate to the top layer coating. Spray the top layer coating 4 times. Dry the coating in the shade at room temperature for 16 hours, and then cure it at 80°C for 24 hours to obtain the coating.
[0175] The coating prepared in this comparative example: a) metallic appearance, uniform surface, no blistering, no cracks, no shedding; b) thickness: 182-196 μm (bottom layer 121-126 μm + middle layer 20-24 μm + surface layer 41-46 μm); c) solar absorption ratio: 0.15; d) hemispherical emissivity: 0.16; e) thermal cycle performance: after -196℃~150℃, 100 times normal pressure thermal cycle test, the coating has uniform appearance color, no obvious color difference, no shedding, and stable thermal physical properties; f) heat resistance: after 180s of high temperature and high speed pneumatic scouring, the coating cracks and peels, and the coating is visible. Figure 4 ; g) Thermal insulation performance: The thermal conductivity of the coating is 0.157W / m·k at room temperature; h) Waterproof performance: The water absorption rate of the coating is 0.4% after being exposed to rain for 24 hours; i) The adhesion of the coating is better than level 1 using the cross-cut test.
[0176] In summary, the structural design of the low-absorption, low-emission thermal control coating resistant to aerodynamic thermal environments of the present invention can obtain a thermal control coating that has good low-absorption, low-emission thermal control performance while being stable in complex aerodynamic thermal environments; at the same time, through the coating structure design and the use of fillers with specific types and proportions, an integrated coating that has good interlayer bonding strength of the multi-layer structure, low-absorption, low-emission thermal control performance, and is heat-resistant, heat-insulating and water-resistant can be obtained.
[0177] Without being limited by any theory, the structural design analysis is as follows: adding hollow glass microsphere powder to the bottom coating can significantly improve the thermal insulation performance of the coating due to the characteristics of hollow glass microspheres. However, after the thermal insulation performance of the bottom layer is improved, the heat transmitted from the outside is prevented from being conducted downward. At the same time, since the composite coating is a low-absorption and low-emission thermal control coating, it has a certain thermal insulation ability. When the external heat enters the coating, it is difficult to dissipate outward through radiation heat dissipation, so a large amount of heat accumulates on the bottom surface. However, the low-absorption and low-emission thermal control surface layer is an organic system with low heat resistance. Therefore, the accumulated heat causes damage to the thermal control surface layer, making it impossible for the coating to pass through the high-temperature, high-speed, and aerodynamic thermal ablation environment while meeting the thermal control performance. Therefore, by matching the bonding strength, heat resistance and thermal conductivity of the coating's multi-layer structure, an organic middle layer is added to make the middle layer have a relatively high thermal conductivity and heat resistance, which plays a role in quickly conducting heat between the surface layer and the bottom layer. At the same time, by adding high-temperature resistant fillers such as alumina with relatively high specific heat capacity, the thermal capacity and heat resistance of the coating are improved, and the heat accumulated in the surface layer is dispersed, thereby ensuring the stability of the low-absorption and low-emission thermal control performance of the composite coating in a high temperature environment.
[0178] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0179] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A low-absorption and low-emission thermal control coating resistant to aerodynamic erosion, characterized in that: Including primer, middle layer and top layer; (I) The primer includes the following raw materials in parts by weight: Component unit A: Component unit B includes ethylene glycol and hollow glass microspheres. The amount of hollow glass microspheres added to solution B is 25-30% of the volume of component unit A, and the amount of ethylene glycol added is 25-30% of the volume of component unit A. (II) The middle layer coating comprises the following raw materials in parts by weight: Component unit A: Component unit B includes curing agent I; (III) The surface coating comprises the following raw materials in parts by weight: Component unit A: Component unit B includes a curing catalyst and a curing agent II.
2. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 1, characterized in that: The silicate aqueous solution in the primer is at least one of a potassium silicate aqueous solution or a lithium silicate aqueous solution, with a mass concentration of 25 to 35%; and / or The powder is at least one of zirconium oxide, zinc oxide or zinc titanate.
3. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 1, characterized in that: The mass concentration of the silica sol in the primer is 20% to 40%; and / or The silane coupling agent is at least one of KH550 and KH560.
4. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 1, characterized in that: The methylphenyl silicone resin in the middle layer coating is a hydroxyl-terminated methylphenyl silicone resin.
5. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 1, characterized in that: The filler in the middle layer coating is a mixed filler of aluminum oxide, titanium oxide, silicon carbide and mica powder, based on 100 parts by mass of methylphenyl silicone resin, there are 50 to 90 parts by mass of aluminum oxide, 50 to 90 parts by mass of titanium oxide, 10 to 20 parts by mass of silicon carbide and 30 to 50 parts by mass of mica powder.
6. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 1, characterized in that: The organic silicon resin in the surface coating is at least one of polydimethylsilicone resin or polydimethylsilicone rubber; and / or The diameter of the aluminum flake powder is 40 to 60 μm; and / or The silane coupling agent is at least one of KH550 and KH560; and / or The curing catalyst is dibutyltin dilaurate; and / or Curing agent II is ethyl orthosilicate.
7. A method for preparing the aerodynamic erosion resistant low absorption and low emission thermal control coating according to any one of claims 1 to 6, characterized in that: include: A silicate aqueous solution, deionized water, silica sol, a silane coupling agent and zinc powder are mixed and ball-milled to form a component unit A; Adding ethylene glycol to the hollow glass microspheres to uniformly wet the hollow glass microspheres to obtain component unit B; mixing component unit B with component unit A to obtain a uniformly dispersed base coating; The methylphenyl silicone resin and the solvent are mixed evenly, fillers and glass beads are added, sand milled and stirred, and curing agent I is added before preparing the coating to obtain a uniformly dispersed middle layer coating; Add solvent, flaky aluminum powder and silane coupling agent to the silicone resin, mix and stir to evenly disperse the filler, add curing agent II and curing catalyst before preparing the coating to obtain an evenly dispersed surface coating.
8. A low-absorption and low-emission thermal control coating resistant to aerodynamic erosion, characterized in that: The low-absorption and low-emission thermal control coating resistant to aerodynamic erosion as claimed in any one of claims 1 to 7 is used to form a composite coating of a bottom layer, a middle layer and a surface layer.
9. The aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 8, characterized in that: The thickness of the bottom layer is 100-200 μm, the thickness of the middle layer is 20-40 μm, and the thickness of the surface layer is 40-50 μm.
10. A method for preparing the aerodynamic erosion resistant low absorption and low emission thermal control coating according to claim 8 or 9, characterized in that: include: The base material surface is sprayed with a primer, and after the primer is cured, the middle layer is sprayed with the middle layer. After the middle layer is cured, the surface layer is sprayed with the top layer. After baking and curing, a low-absorption and low-emission thermal control coating resistant to aerodynamic erosion is obtained.
11. An application of the aerodynamic erosion-resistant, low-absorption, low-emission thermal control coating as described in claim 8 or 9 as a thermal control coating for an on-orbit segment of a spacecraft, or as a rainproof and anti-corrosion coating on the surface of a spacecraft cabin in the absence of a rocket fairing during the launch waiting phase, or as an aerodynamic erosion-resistant coating on the surface of a spacecraft cabin in the absence of a rocket fairing during the rocket launch ascent phase.
Citation Information
Patent Citations
Environment-friendly thermal-insulation anticorrosion coating and coating process thereof
CN102774113A
Spray coating type low-absorption and low-emission thermal control coating, preparation method thereof and application thereof
CN106566408A
A stainresistant thermal barrier paint and a painting process using the same
KR101005045B1
Thermal insulation coating
US20210380840A1