Calcium treatment method for ultra-low carbon molten steel
By using silicon calcium barium alloy to modify Al2O3 in ultra-low carbon steel, spherical calcium aluminate is formed to easily remove, which solves the problem of poor castability of molten steel and improves casting efficiency and molten steel quality.
Patent Information
- Application Number
- CN202411201973.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
In the casting process of ultra-low carbon steel, Al2O3 inclusions with high aluminum content can easily cause water outlets to be blocked, affecting smooth production, and it is difficult for the prior art to effectively improve the castability of the steel.
Use silicon calcium barium alloy as deoxidant and desulfurizer. By adding aluminum blocks, manganese metal and ferrosilicon to the RH furnace, the vacuum degree and temperature are controlled, the vacuum pump is turned off step by step, and the silicon calcium barium alloy is put into the silicon to modify the Al2O3 in the molten steel. , forming spherical calcium aluminate that is easy to remove, and improving the water-soakability of molten steel.
It effectively improves the castability of ultra-low carbon steel, reduces the oxidation and vapor pressure of calcium, improves the solubility of calcium, reduces temperature drop and steam consumption, increases the number of castings, and solves the problem of water outlet clogging.
Smart Images

Figure BDA0005018063020000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for treating ultra-low carbon molten steel with calcium. Background Art
[0002] In the prior art, ultra-low carbon molten steel with a high aluminum content often has nozzle blockage during the casting process, which has a great impact on the smooth production. The CSP line continuous casting adopts an integral tundish and the nozzle cannot be replaced. The fine dispersed Al2O3 in the ultra-low carbon steel will gather at the stopper rod and affect the castability of the molten steel. The Al2O3 inclusions in the molten steel are modified by calcium treatment of the molten steel, thereby improving the castability of the molten steel.
[0003] The patent application with publication number CN 104946851 A discloses a smelting method that can make O≤0.001% in ultra-low carbon molten steel in a vacuum induction furnace. The inclusions in the steel are denatured by calcium treatment, so that they aggregate, grow, float and are removed. The inclusions in the steel are adsorbed by slag making, so that the S in the steel is removed to less than 0.001%. The smelting method of ultra-low carbon steel in a vacuum induction furnace can reduce the inclusions in the steel, especially the large particle inclusions. However, how to modify the inclusions in the steel to improve the castability of the molten steel is still a difficult problem that needs to be solved today. Summary of the invention
[0004] The object of the present invention is to provide a method for treating ultra-low carbon molten steel with calcium, which improves the castability of CSP ultra-low carbon steel and improves the efficiency by modifying the Al2O3 inclusions in the ultra-low carbon molten steel.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for treating ultra-low carbon molten steel with calcium comprises the following steps:
[0007] (1) Converter blowing: The molten iron with a sulfur content of ≤0.005% after desulfurization treatment and clean scrap steel are poured into the converter for oxygen blowing smelting. During the steel tapping process, high carbon ferromanganese is added for alloying and argon gas is passed for stirring;
[0008] (2) RH furnace refining: When the molten steel enters the RH furnace, the RH vacuum valve is opened, oxygen is blown to reduce the carbon content of the molten steel, and then the temperature is measured and sampled, and aluminum blocks, metallic manganese and ferrosilicon are added; then the vacuum pump is closed step by step, and the vacuum degree in the RH furnace is controlled at 9-11Kpa; silicon-calcium-barium alloy is added through the silo, and the steel is emptied and discharged after circulation. Samples are taken before emptying to test the calcium content of the molten steel.
[0009] (3) Continuous casting: The molten steel enters the continuous casting table and is cast according to the target casting speed.
[0010] Furthermore, the desulfurization treatment is one of KR desulfurization and powder spraying desulfurization.
[0011] Furthermore, the sulfur content of the desulfurization treatment is ≤0.001%.
[0012] Furthermore, the mass ratio of the molten iron to the clean scrap steel is 75-85:20-25.
[0013] Furthermore, the amount of high carbon ferromanganese added is 50-65kg.
[0014] Furthermore, the argon gas flow rate is 300NL / min.
[0015] Furthermore, the RH vacuum valve reduces the vacuum degree in the furnace to ≤133Pa.
[0016] Furthermore, the carbon content of the molten steel is ≤0.002%.
[0017] Furthermore, the temperature of the temperature measurement sampling is 1575-1610°C.
[0018] Furthermore, the mass ratio of the aluminum block, metallic manganese and ferrosilicon is 400-450:50-70:850-950.
[0019] Furthermore, the silicon-calcium-barium alloy comprises the following components in percentage by weight: Ca≥12.5%, Ba≥13.5%, Si≥52%, P≤0.1%, S≤0.15%, C≤1.0% and the balance Fe.
[0020] Furthermore, the addition amount of the silicon-calcium-barium alloy is 10-30 kg.
[0021] Furthermore, the cycle time is 1 to 3 minutes.
[0022] Furthermore, the target pulling speed is 3.6-4.8 m / min, and the pulling speed is constant during casting.
[0023] Beneficial effects of the present invention:
[0024] (1) The silicon-barium-calcium alloy used in the present invention as a steelmaking deoxidizer and desulfurizer mainly consists of silicon, barium, calcium and other elements. It is a new type of composite deoxidizer in barium alloys and is often used as a deoxidizer for steelmaking. It also has the functions of desulfurization and dephosphorization. After silicon-calcium-barium is added to molten steel, the aluminum oxide inclusions in the molten steel can be modified into spherical calcium aluminates such as CA6, CA2, C12A7, which are easier to remove from the molten steel.
[0025] (2) Barium effectively reduces the vapor pressure of calcium within the steelmaking temperature range and increases the solubility of calcium in molten steel. After adding silicon-calcium-barium alloy, completing one RH pump-back process cycle (about 1.5-2 minutes) and leaving the station with uniform composition can preserve the calcium content in the molten steel to the greatest extent, thereby achieving the purpose of calcification treatment of the molten steel by reducing calcium oxidation.
[0026] (3) The present invention adopts the RH pump-back process, which does not require breaking the slag surface to feed the calcium line, reducing the temperature drop by 8-10°C and reducing the RH steam consumption by 0.01t / ton of steel. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a method for treating ultra-low carbon molten steel with calcium, comprising the following steps:
[0030] The smelting equipment used in this embodiment is a nominal 100-ton converter, and the components of the silicon-calcium-barium alloy are, by weight percentage, 14.7% Ca, 13.9% Ba, 53.1% Si, 0.04% P, 0.09% S, 0.22% C and 17.95% Fe.
[0031] (1) Converter blowing: 80 tons of molten iron with a sulfur content of ≤0.001% after KR desulfurization treatment and 20 tons of clean scrap steel are poured into the converter for oxygen blowing smelting. During the steelmaking process, 60 kg of high carbon ferromanganese is added for deoxidation and alloying, and argon is passed for stirring at an argon flow rate of 300 NL / min.
[0032] (2) RH furnace refining: When the molten steel enters the RH furnace, the RH vacuum valve is opened until the vacuum degree in the furnace is ≤133Pa, oxygen is blown to reduce the carbon content of the molten steel to less than 0.002%, and then the temperature is measured and sampled. 420kg of aluminum blocks, 60kg of metallic manganese, and 900kg of ferrosilicon are added to achieve the target composition. After the composition reaches the target, the vacuum pump is retreated to level 5. At this time, the vacuum degree in the RH furnace is 9-11Kpa. 20kg of silicon-calcium-barium alloy is added through the silo, and the furnace is circulated for 1.5 minutes under the level 5 pump before breaking the vacuum. Samples are taken to test the calcium content of the molten steel before breaking the vacuum.
[0033] (3) Continuous casting: The molten steel enters the continuous casting table and is cast according to the target casting speed.
[0034] Example 2
[0035] The present embodiment is different from the embodiment 1 in that 30 kg of silicon-calcium-barium alloy is added, and the components of the silicon-calcium-barium alloy are, by weight percentage, 14.1% Ca, 14.2% Ba, 53.2% Si, 0.06% P, 0.03% S, 0.17% C and 18.24% Fe.
[0036] The remaining raw materials and preparation process remain the same as in Example 1.
[0037] Comparative Example 1
[0038] The difference between this comparative example and Example 1 is that in step (2), the vacuum pump is set back to level 3. The specific implementation steps are as follows:
[0039] (2) RH furnace refining: When the molten steel enters the RH furnace, the RH vacuum valve is opened until the vacuum degree in the furnace is ≤133Pa, oxygen is blown to reduce the carbon content of the molten steel to less than 0.002%, and then the temperature is measured and sampled. 407kg of aluminum blocks, 58kg of metallic manganese, and 909kg of ferrosilicon are added to achieve the target composition. After the composition reaches the target, the vacuum pump is retreated to level 3. At this time, the vacuum degree in the RH furnace is 1-3Kpa. 20kg of silicon-calcium-barium alloy is added through the silo, and the furnace is circulated under the level 3 pump for 1 minute and 10 seconds before breaking the vacuum. Samples are taken to test the calcium content of the molten steel before breaking the vacuum.
[0040] The remaining raw materials and preparation process remain the same as in Example 1.
[0041] Comparative Example 2
[0042] The difference between this comparative example and Example 1 is that no silicon-calcium-barium alloy is added.
[0043] The remaining raw materials and preparation process remain the same as in Example 1.
[0044] Comparative Example 3
[0045] Compared with Example 1, the difference between this comparative example and Example 1 is that "20 kg of silicon-calcium-barium alloy" is replaced by "20 kg of silicon-calcium alloy". The components of the silicon-calcium alloy are 27.53% Ca, 55.03% Si, 0.02% P, 0.04% S, 0.45% C, 1.54% Al and 15.39% Fe in weight percentage.
[0046] The remaining raw materials and preparation process remain the same as in Example 1.
[0047] Comparative Example 4
[0048] The difference between this comparative example and Example 1 is that "20kg silicon-calcium-barium alloy" is replaced with "50kg silicon-calcium alloy". (Silicon-calcium alloy is the same as that in comparative example 3)
[0049] The remaining raw materials and preparation process remain the same as in Example 1.
[0050] The calcium content of molten steel before breaking and the number of continuous castings were tested for Example 1-Example 2 and Comparative Example 1-Comparative Example 4, and the results are shown in Table 1:
[0051] Table 1
[0052]
[0053] It can be seen from Table 1 that, compared with Example 1, when the vacuum degree in the RH furnace is only 1-3 KPa, even if enough silicon-barium-calcium alloy is added, the calcium content is extremely low and the number of continuous castings is far less than that in Example 1.
[0054] Compared with Example 1, the addition amount of barium element is reduced in Comparative Examples 2-4, and the calcium content of molten steel is also reduced accordingly, because barium effectively reduces the vapor pressure of calcium within the steelmaking temperature range and increases the solubility of calcium in molten steel. Compared with silicon-calcium alloy, when silicon-barium-calcium alloy is used as a calcium source and added to molten steel, the calcium content in molten steel can reach about twice the calcium content when silicon-calcium alloy is used, and the calcium content in molten steel is also significantly increased. It is fully demonstrated that barium effectively protects calcium in molten steel and reduces calcium oxidation, thereby achieving the purpose of calcification treatment of molten steel. The reduction in the number of pouring times is because the fine dispersed Al2O3 in ultra-low carbon steel will gather at the stopper rod and cause blockage of the water outlet. After adding silicon-calcium-barium alloy to molten steel, the aluminum oxide inclusions in the molten steel can be modified into spherical calcium aluminates such as CA6, CA2, and C12A7, which are easier to remove from the molten steel, thereby increasing the number of pouring times.
[0055] In summary, the method for calcium treatment of ultra-low carbon molten steel provided by the present invention has good application prospects in the field of steel smelting technology.
[0056] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for treating ultra-low carbon molten steel with calcium, characterized in that: The steps include: (1) Converter blowing: pouring molten iron with a sulfur content of ≤0.005% after desulfurization treatment and clean scrap steel into a converter for oxygen blowing smelting; adding high carbon ferromanganese for alloying during the steel tapping process and stirring with argon gas; (2) RH furnace refining: The molten steel enters the RH furnace, the RH vacuum valve is opened, oxygen is blown to reduce the carbon content of the molten steel, and then the temperature is measured and sampled, and aluminum blocks, metallic manganese and ferrosilicon are added; then the vacuum pumps are closed step by step to control the vacuum degree in the RH furnace at 9-11Kpa; silicon-calcium-barium alloy is added through the silo, and after circulation, it is broken through the air and discharged from the station.
2. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The desulfurization treatment is one of KR desulfurization and powder spray desulfurization; the sulfur content of the desulfurization treatment is ≤0.001%.
3. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The mass ratio of the molten iron to the clean scrap steel is 75-85:20-25; the added amount of the high carbon ferromanganese is 50-65kg.
4. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The argon gas flow rate is 300NL / min.
5. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The RH vacuum valve reduces the vacuum degree in the furnace to ≤133Pa.
6. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The carbon content of the molten steel is ≤0.002%.
7. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The temperature of the temperature measurement sampling is 1575-1610°C.
8. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The mass ratio of the aluminum block, metallic manganese and ferrosilicon is 400-450:50-70:850-950.
9. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The silicon-calcium-barium alloy comprises the following components in percentage by weight: Ca≥12.5%, Ba≥13.5%, Si≥52%, P≤0.1%, S≤0.15%, C≤1.0% and the balance Fe; the addition amount of the silicon-calcium-barium alloy is 10-30kg.
10. The method for treating ultra-low carbon molten steel with calcium according to claim 1, characterized in that: The cycle time is 1 to 3 minutes.
Citation Information
Patent Citations
Smelting method capable of lowering O in ultra-low carbon steel water in vacuum induction furnace to be no greater than 0.001 percent
CN104946851A