Thin-gauge 590MPa-grade low-cost high-surface-quality automobile chassis steel produced by CSP production line and method thereof
Through low Mn, low Nb, and extremely low Si composition design and CSP process optimization, combined with casting billet heating and winding temperature control, the shortcomings of automotive chassis steel in terms of hole reaming and flanging performance and surface quality are solved, and a 590MPa level is achieved The extremely low-cost and high-surface quality steel for automotive chassis meets the automotive industry's demand for high strength, good reaming and flange performance and high surface quality.
Patent Information
- Application Number
- CN202411200172.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing steels for automotive chassis parts have shortcomings in terms of reaming and flanging performance and surface quality. The high Mn and Nb of traditional duplex steel components lead to increased costs, and the Si element inhibits the precipitation of cementite but affects the surface quality, which cannot meet the needs of automotive chassis parts. Demand for high strength, good reaming and flange performance and high surface quality.
Using chemical composition design with low Mn content, low Nb content and extremely low Si content, combined with CSP thin slab continuous casting and rolling process, the high tensile strength, yield strength and Elongation and optimize surface quality through pickling process to form bainite + ferrite structure of fine grains.
The steel plate tensile strength of the steel plate is ≥590MPa, yield strength ≥440MPa, elongation ≥24%, and porosity reaming ≥120%, and the production cost is reduced to meet the automotive chassis Parts require high reaming flange performance and surface quality.
Smart Images

Figure BDA0005017654110000061 
Figure BDA0005017654110000062 
Figure BDA0005017654110000071
Abstract
Description
Technical Field
[0001] The invention belongs to the field of pickling high-performance automobile steel, and specifically relates to a method for producing thin-gauge 590MPa grade extremely low-cost and high-surface-quality automobile chassis steel using a CSP production line and a product thereof. Background Art
[0002] The automotive industry in the 21st century will reduce fuel consumption and CO 2 And exhaust emissions have become a social need. In order to adapt to this development trend, the steel industry as a material manufacturer has developed many types of ultra-high strength steel plates to help reduce the weight of cars and adapt to the new requirements of the automotive industry.
[0003] As an important part of automobile parts, automobile chassis parts require steel materials with high strength and thinning. In order to meet the needs of assembly and use, more round holes are usually designed on the parts. These round holes need to be punched first and then expanded and flanging to obtain the final parts during the forming process. A large amount of data shows that the expansion performance of materials is not completely equivalent to the forming performance. Generally speaking, the better the plasticity of steel, the better the forming performance, but it does not necessarily mean that the expansion and flanging performance is better. For example, traditional dual-phase steel has good plasticity and good forming performance, but its expansion and flanging performance is poor, which is not suitable for the production of automobile suspension parts and chassis parts that require expansion. Therefore, for the growing automobile industry, the requirements for automobile chassis parts are becoming more and more stringent. Not only high strength and high plasticity are required, but also good expansion and flanging performance and good surface quality requirements. The thinnest thickness of pickled steel plates after high strength and thinning is required to reach 1.5mm. At the same time, in order to meet the cruel market competition, cost control has become the lifeline of all automobile manufacturers.
[0004] CN117248161A discloses a 600MPa grade low-cost pickled automobile steel plate with high hole expansion performance, the chemical composition and weight percentage content of which are: C 0.035%-0.065%, Si 0.30%-0.65%, Mn 1.40%-1.65%, Nb0.020%-0.030%, Ti 0.010%-0.025%, P≤0.010%, S≤0.004%, and the rest are Fe and unavoidable impurities. However, more than 1.4% Mn and more than 0.020% Nb are added to the steel plate. In the current increasingly competitive market environment, the extremely low-cost composition design can better meet market demand. In addition, the addition of Si element inhibits the precipitation of cementite and increases the hole expansion rate. However, the addition of Si will affect the surface quality and form tiger skin patterns on the surface of the hot-rolled plate, which cannot fully meet the surface quality requirements of automobile chassis parts. In addition, in order to reduce the risk of tiger skin pattern defects caused by high Si content, high-pressure water descaling is required before rolling, which will also increase the process cost. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides a thin-gauge 590MPa-grade steel for automobile chassis with extremely low cost and high surface quality, specifically with a thickness of 1.0mm to 5.0mm. After pickling, the tensile strength of the steel plate is ≥590MPa, the yield strength is ≥440MPa, the elongation is ≥24%, the hole expansion rate is ≥120%, and it has good surface quality, meeting the requirements of automobile chassis parts for hole expansion and flanging performance.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A thin-gauge 590MPa grade steel for automobile chassis with extremely low cost and high surface quality, which is designed with a composition having low Mn content, low Nb content and extremely low Si content, and has the following composition and weight percentage: C 0.034-0.059%, Si 0.03-0.14%, Mn 0.64-0.97%, Nb 0.012-0.020%, Ti 0.031-0.057%, N≤0.005%, S≤0.004%, and the rest being Fe and unavoidable impurities.
[0008] Preferably, the weight percentage of C is 0.038-0.055%.
[0009] Preferably, the weight percentage content of Si is 0.06-0.11%.
[0010] Preferably, the weight percentage of Mn is 0.65-0.90%.
[0011] Preferably, the weight percentage content of Ti is 0.035-0.053%.
[0012] The present invention also provides a method for producing thin-gauge 590MPa grade extremely low-cost high-surface quality automobile chassis steel, which is produced by CSP thin slab continuous casting and rolling process. The process flow includes: molten iron desulfurization, smelting and refining, continuous casting, billet heating, rolling, cooling, coiling and pickling, etc. The specific steps are as follows:
[0013] 1) Desulfurizing, smelting and refining molten iron to obtain molten steel with target composition;
[0014] 2) After refining, continuous casting is carried out, and the superheat of the molten steel in the tundish is controlled at 15-30°C, the thickness of the cast billet is 57-65mm, and the casting speed is 4.0-4.6m / min;
[0015] 3) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1240°C;
[0016] 4) Rolling is performed without high-pressure water descaling before rolling. The first pass reduction rate is controlled to be 52-63%, the second pass reduction rate is 50-60%, and the final pass reduction rate is 10-16%; the rolling speed is controlled to be 8-12 m / s; medium-pressure water descaling is performed between the first and second passes, and the descaling water pressure is 200-280 bar; the final rolling temperature is controlled to be 860-900° C.;
[0017] 5) Cooling is carried out by front-stage cooling method, and the front-stage cooling rate is ≥120℃ / s;
[0018] 6) Coil the coil, and the coiling temperature is dynamically matched with the effective Ti, and the coiling temperature is controlled to be 500-1020*[effective Ti]), in ° C; wherein, [effective Ti]=[Ti]-3*[S]-3.42*[N], [Ti], [S], [N] are the weight percentage contents of Ti, S, and N in the steel composition respectively;
[0019] 7) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
[0020] Preferably, the temperature of the ingot entering the furnace is controlled at 835-910°C, the time in the furnace is controlled at 25-35 minutes, and the temperature out of the furnace is controlled at 1210-1233°C.
[0021] The thin-gauge 590MPa grade steel for automobile chassis with extremely low cost and high surface quality produced by the above method has a thickness of 1.0mm to 5.0mm, a tensile strength of ≥590MPa, a yield strength of ≥440MPa, an elongation of ≥24%, and a limit hole expansion rate of ≥120%; the metallographic structure is a bainite + ferrite structure with fine grain size, and the grain size grade is ≥10. Further preferably, the thickness is 1.0mm to 4.0mm, the tensile strength of the steel plate is ≥615MPa, the yield strength is ≥490MPa, the elongation is ≥25%, the limit hole expansion rate is ≥125%, and the pickling streak color difference defect degradation rate does not exceed 0.2%; the metallographic structure is a bainite + ferrite structure with fine grain size, and the grain size grade is ≥10.5.
[0022] The functions and mechanisms of various raw materials and main processes in the present invention are:
[0023] C: In order to ensure that the steel plate obtains a tensile strength of more than 590MPa, the carbon content of the present invention must be at least 0.034%, otherwise the tensile strength of the plate is difficult to meet the requirements. At the same time, the C content has a significant effect on the hole expansion performance. The higher the C content, the easier it is to generate cementite and pearlite. These structures are not conducive to improving the hole expansion performance. In order to improve the hole expansion rate and ensure the strength, the C content is controlled in the range of 0.034-0.059%, preferably 0.038-0.055%.
[0024] Si: Si can effectively inhibit the precipitation of cementite, which has an adverse effect on hole expansion performance. Therefore, in order to improve the hole expansion performance, the usual high hole expansion steel adds 0.30% Si to effectively inhibit the precipitation of cementite and improve the hole expansion performance. However, when the Si content exceeds 0.15%, the hot-rolled steel plate is prone to produce tiger stripes, and even after pickling, stripes will appear, affecting the surface quality of the steel plate. The important innovation of the present invention is to add a small amount or trace amount of Si element so that the steel plate can obtain good surface quality. The Si content of the present invention is controlled at 0.03-0.14%, preferably 0.03-0.11%.
[0025] Mn: Mn is the most effective element for improving strength and toughness, and is also one of the important alloying elements used in the present invention. Mn can stabilize austenite and reduce the critical quenching rate of steel, thereby improving the hardenability of the material. The Mn content of conventional 590MPa-grade high-strength steel is above 1.0%, generally around 1.5%. The present invention adopts an extremely low-cost component design, and the Mn content is controlled at 0.64-0.97%, preferably 0.65-0.90%. Compared with the traditional 590MPa-grade high-strength steel with a Mn content of 1.5%, the cost per ton of steel of the present invention can be reduced by 80-140 yuan, which is equivalent to a reduction of about 3% in the cost of the finished product.
[0026] S: S is an impurity element in steel. If the sulfur content is too high, it will increase the hot brittleness tendency of the steel. S in steel often exists in the form of manganese sulfide. This sulfide inclusion is very unfavorable to the impact toughness of steel and causes anisotropy of performance. Therefore, the sulfur content in steel needs to be controlled as low as possible. Therefore, the sulfur content in steel is controlled below 0.004%.
[0027] N: N is an impurity element in steel. If the N content is too high, it will form large particles of TiN with the Ti element in the steel, thereby reducing the precipitation strengthening effect and fine grain strengthening effect of Ti. Therefore, the lower the nitrogen content, the better. In actual production, it is generally controlled below 0.005%.
[0028] Nb: Nb is one of the important alloying elements used in the present invention. Adding Nb element can effectively refine the original austenite grain size and improve the strength and plasticity of the steel plate; in addition, the refined bainite structure can effectively inhibit the expansion of cracks during the hole expansion and flanging process and improve the hole expansion rate; if the Nb content exceeds 0.020%, it will lead to an increase in alloy cost. Therefore, the Nb content of the present invention is controlled at 0.012-0.020%.
[0029] Ti: Ti is one of the important alloying elements used in the present invention. Ti can play a role in fine grain strengthening and precipitation strengthening. In the present invention, 0.031% of Ti element is added to replace the strengthening effect of Mn element; at the same time, the alloy cost of Ti element is very low, realizing an extremely low-cost design; if the Ti element content is too high, the number of coarse carbide and nitride inclusions will increase, thereby affecting the comprehensive mechanical properties. Therefore, the Ti content of the present invention should be controlled at 0.031-0.057%, preferably 0.035-0.053%.
[0030] In addition to limiting the range of the above chemical components, from the perspective of improving the formability and economy of the material, the present invention does not add precious alloy elements such as Mo, V, Cu, and Ni, and achieves extreme low cost by reducing the Mn content and Nb content, adding a small amount of relatively cheap Ti and limiting S and N, so that the added Ti can fully play the purpose of precipitation strengthening and fine grain strengthening; and because the present invention adopts a low Si component design, high-pressure water descaling before rolling is not required. According to the above changes in component design, the present invention designs the drawing speed of the continuous casting billet, the billet heating process, and the coiling addition, so that the added Ti can not only make up for the strength loss after reducing Mn and Nb through precipitation strengthening, but also refine the grains by controlling the size of the precipitates to make up for the reduction in the hole expansion rate after reducing Si.
[0031] The present invention increases the furnace temperature of the ingot to 1200-1240°C, and the furnace time is 20-40min, so as to ensure that the temperature of the steel plate during the steel rolling process meets the requirements of each link. In order to cooperate with the reduction of Mn and the increase of Ti, in order to ensure the precipitation and fine grain strengthening effect of Ti, the present invention specifically studies the heating temperature of the ingot, and the heating temperature has a very important influence on the various properties of the finished product, and the heating temperature must be guaranteed to be above 1200°C. When the heating temperature is too low and the furnace time is too short, the Ti in the ingot cannot be completely dissolved, and in the subsequent rolling and cooling process, it is impossible to precipitate enough fine and dispersed precipitates, and the requirements of strength and hole expansion rate cannot be met; however, when the heating temperature is too high and the furnace time is too long, the original austenite grains before rolling will be coarse, which will cause the subsequent rolling process to fail to complete the complete recrystallization process of austenite, which will cause mixed crystals in the final product (i.e., the product grain size is uneven), which will seriously affect the product quality.
[0032] The coiling temperature of the present invention adopts a process of dynamically matching the effective Ti content. This is because Ti is an active element and has a great influence on mechanical properties including strength and hole expansion rate. Ti is easily combined with S and N in steel to form large particles of TiS and TiN. Such precipitates cannot make a positive contribution to strength and hole expansion rate. [Effective Ti] is generally used to evaluate the actual effect of Ti. [Effective Ti] = [Ti] - 3 * [S] - 3.42 * [N]. Effective Ti is in the range of 0.012 to 0.035%. The present invention sets the coiling temperature according to the actual value of [Effective Ti] and obtains the best mechanical properties through dynamic matching. The coiling temperature = 500-1020 * [Effective Ti]), in units of ° C.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention adopts reasonable chemical composition, does not add precious alloy elements such as Mo, V, Cu, Ni, etc., and adopts a composition design with low Mn content, low Nb content and extremely low Si content to meet the requirements of extremely low cost and high surface quality, and ensures the performance requirements of the material by adding a certain amount of relatively low-cost Ti. On this basis, the present invention combines the optimization of the heating temperature and time of the ingot and accurately matches the coiling temperature according to the effective Ti, so that the precipitation strengthening and fine grain strengthening effects of Ti are maximized, and high strength can be obtained through various strengthening effects, and high elongation and high hole expansion rate can be obtained through fine grain ferrite and bainite structures, and the requirements of high strength, high elongation and high hole expansion rate can still be met at the same time, and finally 590MPa grade extremely low-cost high surface quality automobile chassis steel can be obtained, which can achieve a bainite + ferrite structure with a fine grain size and a grain size grade of ≥10; and ensure that the tensile strength of the steel plate is ≥590MPa, the yield strength is ≥440MPa, the elongation is ≥24%, the hole expansion performance is excellent, the hole expansion rate is ≥120%, and the pickling stripe color difference defect degradation rate does not exceed 0.2%. Compared with the traditional 590MPa grade high hole expansion steel, the present invention adopts an extremely low-cost component design and has excellent surface quality, which can still meet the requirements of automobile chassis parts for surface quality and high hole expansion and flanging performance, and further reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the metallographic structure diagram (bainite + ferrite) of the 590MPa grade extremely low-cost and high-surface quality pickled steel plate for automobile chassis of the present invention. DETAILED DESCRIPTION
[0036] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0037] In the present invention, the hole expansion test is carried out according to the national standard requirements. A center hole of d=10 mm is punched in the center of a 150mm*150mm square plate. A conical hole expansion punch of a specified shape and size is pushed into the punched circular hole of a metal dark plate sample to carry out the hole expansion test until a crack penetrating the thickness of the sample appears at the edge of the circular hole. The punch is stopped and the limit hole expansion rate is measured. Hole expansion rate λ= Where λ is the limit hole expansion rate, %; D 0 is the initial diameter of the punched hole (D 0 =10mm); D H is the average diameter of the circular holes after rupture, in millimeters (mm). The hole expansion rate of the steel plate prepared by the present invention can reach more than 120%.
[0038] Example
[0039] The following describes each embodiment in detail:
[0040] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0041] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0042] Table 3 is a list of performance test results of various embodiments of the present invention and comparative examples; wherein the test standards for strength and elongation are GB / T 223, and the test standard for hole expansion rate is GB / T 24524.
[0043] Each embodiment of the present invention produces thin-gauge 590MPa grade extremely low-cost and high-surface quality automobile chassis steel according to the following steps, and the specific steps are as follows:
[0044] 1) Desulfurization of molten iron, desulfurization target: S≤0.001%, the exposed surface of molten iron after slag removal is not less than 95%;
[0045] 2) Conventional converter smelting and conventional refining to obtain molten steel with target composition;
[0046] 3) After smelting, continuous casting is carried out, and the superheat of the molten steel in the tundish is controlled at 15-30°C, the thickness of the billet is 57-65mm, and the billet drawing speed is 4.0-4.6m / min;
[0047] 4) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1240°C;
[0048] 5) Rolling, and controlling the first pass reduction rate to be 52-63%, the second pass reduction rate to be 50-60%, and the final pass reduction rate to be 10-16%; controlling the rolling speed to be 8-12 m / s; and performing medium-pressure water descaling between the first and second passes, with the descaling water pressure being 200-280 bar; and controlling the final rolling temperature to be 860-900° C.;
[0049] 6) Use the front-stage cooling method for cooling, and the front-stage cooling rate is ≥120℃ / s;
[0050] 7) Coil the coil and control the coiling temperature = 500-1020*[effective Ti]), the unit is ° C, substitute the effective Ti in Table 1 to obtain the corresponding coiling temperature (Note: when [effective Ti] is substituted into the formula of the coiling temperature, there is no need to substitute the unit %, for example, in Example 1, 0.0208 is substituted into the formula of the coiling temperature, and the coiling temperature = 500-1020*0.0208≈479° C.), as shown in Table 3, in the range of 465-490° C.;
[0051] 8) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
[0052] The production process of the comparative example is carried out with reference to the example, and the specific component values, process parameter values and performance tests are also shown in Tables 1, 2 and 3.
[0053] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0054]
[0055] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0056]
[0057]
[0058] Table 2
[0059]
[0060] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0061]
[0062] Note: The downgrade rate of pickling streak color difference defect refers to the proportion of pickled steel plates judged as downgraded products due to severe streak color difference on the surface.
[0063] It can be clearly seen from Table 3 that by adopting the chemical composition and production process of the present invention, a bainite + ferrite structure with fine grain size is obtained, and the grain size grade is ≥10; the tensile strength of the steel plate is ≥590MPa, the yield strength is ≥440MPa, the elongation is ≥24%, and the hole expansion rate is ≥120%. Compared with the traditional 600MPa grade high-strength steel such as DP600 (the hole expansion rate is only about 60%), the hole expansion performance is significantly improved, and compared with the traditional high hole expansion steel FB590 (the alloy cost is high, there are striped morphology on the surface, and the hole expansion rate is about 80%), the production cost is significantly reduced, the surface quality is improved, and the degradation rate of the pickling stripe color difference defect does not exceed 0.2%. The mechanical properties can also be guaranteed to meet the requirements of the automotive chassis for surface quality and high hole expansion and flanging performance. For example, in Comparative Examples 2 and Comparative Examples 3, a relatively high amount of Si is added, and the hot-rolled steel plate is easy to form tiger stripes, and the pickling stripe color difference defect is formed after pickling, which cannot meet the user's high requirements for surface quality.
[0064] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A thin-gauge 590MPa grade steel for automobile chassis with extremely low cost and high surface quality, characterized in that: The steel adopts a composition design with low Mn content, low Nb content and extremely low Si content. The composition and weight percentage of the steel for automobile chassis are: C 0.034-0.059%, Si 0.03-0.14%, Mn 0.64-0.97%, Nb 0.012-0.020%, Ti 0.031-0.057%, N≤0.005%, S≤0.004%, and the rest are Fe and unavoidable impurities.
2. The thin-gauge 590MPa grade extremely low-cost and high-surface quality automobile chassis steel according to claim 1, characterized in that: The weight percentage of C is 0.038-0.055%.
3. The thin-gauge 590MPa grade extremely low-cost and high-surface quality automobile chassis steel according to claim 1, characterized in that: The weight percentage content of Si is 0.06-0.11%.
4. The thin-gauge 590MPa grade extremely low-cost and high-surface quality automobile chassis steel according to claim 1, characterized in that: The weight percentage of Mn is 0.65-0.90%.
5. The thin-gauge 590MPa grade steel for automobile chassis with extremely low cost and high surface quality according to claim 1, characterized in that: The weight percentage content of Ti is 0.035-0.053%.
6. A method for producing the thin-gauge 590 MPa grade extremely low-cost and high-surface quality automobile chassis steel according to any one of claims 1 to 5, produced by CSP thin slab continuous casting and rolling process, characterized in that: The steps include: 1) Desulfurizing, smelting and refining molten iron to obtain molten steel with target composition; 2) After refining, continuous casting is carried out, and the superheat of the molten steel in the tundish is controlled at 15-30°C, the thickness of the cast billet is 57-65mm, and the casting speed is 4.0-4.6m / min; 3) heating the ingot, and controlling the ingot temperature to be between 800 and 950°C, the ingot time to be between 20 and 40 minutes, and the out-of-furnace temperature to be between 1200 and 1240°C; 4) Rolling is performed without high-pressure water descaling before rolling. The first pass reduction rate is controlled to be 52-63%, the second pass reduction rate is 50-60%, and the final pass reduction rate is 10-16%; the rolling speed is controlled to be 8-12 m / s; Medium pressure water descaling is carried out between the first and second passes, and the descaling water pressure is 200-280 bar; the final rolling temperature is controlled at 860-900℃; 5) Cooling is carried out by front-stage cooling method, and the front-stage cooling rate is ≥120℃ / s; 6) Coil the coil, and the coiling temperature is dynamically matched with the effective Ti, and the coiling temperature is controlled to be 500-1020*[effective Ti]), in ° C; wherein, [effective Ti]=[Ti]-3*[S]-3.42*[N], [Ti], [S], [N] are the weight percentage contents of Ti, S, and N in the steel composition respectively; 7) Perform pickling, and perform continuous pickling at a pickling speed of 100 to 120 m / min.
7. The method for producing thin-gauge 590MPa grade steel for automobile chassis with extremely low cost and high surface quality according to claim 6, characterized in that: The ingot entering furnace temperature is controlled at 835-910℃, the ingot staying time is controlled at 25-35min, and the out-of-furnace temperature is controlled at 1210-1233℃.
8. The automobile chassis steel according to any one of claims 1 to 5 or the automobile chassis steel produced by the method according to claim 6 or 7, characterized in that: The thickness is 1.0mm~5.0mm, the tensile strength of the steel plate is ≥590MPa, the yield strength is ≥440MPa, the elongation is ≥24%, the ultimate hole expansion rate is ≥120%, and the pickling streak color difference defect degradation rate does not exceed 0.2%; the metallographic structure is bainite + ferrite structure, and the grain size grade is ≥10.
9. The automobile chassis steel according to any one of claims 1 to 5 or the automobile chassis steel produced by the method according to claim 6 or 7, characterized in that: The thickness is 1.0mm~4.0mm, the tensile strength is ≥615MPa, the yield strength is ≥490MPa, the elongation is ≥25%, the hole expansion rate is ≥125%, and the degradation rate of the pickling stripe color difference defect does not exceed 0.2%; the metallographic structure is bainite + ferrite structure, and the grain size grade is ≥10.5.
Citation Information
Patent Citations
Hot-rolled high-strength sheet steel having tensile strength of 540MPa, and production method thereof
CN103667908A
600MPa-grade low-cost high-reaming-performance acid pickling automobile steel plate and production method thereof
CN117248161A
High-strength hot rolled steel sheet having excellent stretch flangeability, ductility,and method for manufacturing the same
KR1020090069880A