Nickel-based alloy surface high-temperature-resistant thermal-shock-resistant thermal barrier coating and preparation method thereof

By forming a multi-layer thermal barrier coating on the surface of nickel-based alloy, combined with different spraying techniques and material proportions, the thermal barrier coating of nickel-based alloy thermal barrier coating in the prior art is solved inadequate thermal insulation and thermal shock resistance in high temperature environments in the prior art. The problem of achieving higher thermal insulation and thermal shock resistance.

CN119061345AActive Publication Date: 2024-12-03KUNMING UNIV OF SCI & TECH

Patent Information

Application Number
CN202411194085.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing nickel-based alloy thermal barrier coatings have insufficient thermal insulation and thermal shock resistance in high temperature environments, especially when the bonding strength decreases during the alternation of hot and cold, resulting in weak thermal shock resistance.

Method used

The thermal barrier coating consisting of the first bonding layer, the second bonding layer, the ceramic transition layer and the ceramic layer are used, and vacuum plasma spraying and supersonic flame spraying technology are used respectively, combining the different proportions of RETaO4 and YSZ or Gd2Zr2O7 materials, A dense bonding layer and a ceramic layer are formed to improve high temperature resistance and thermal shock resistance.

Benefits of technology

It significantly improves the thermal insulation performance and thermal shock resistance of the nickel-based alloy surface. It can insulate the maximum temperature at 1500℃ to 437℃, and the number of water quenchings reaches 347 times after 10 minutes of insulation at 1200℃, which is significantly better than the current one. Have technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061345A_ABST
    Figure CN119061345A_ABST
Patent Text Reader

Abstract

The invention discloses a nickel-based alloy surface high-temperature-resistant thermal-shock-resistant thermal barrier coating and a preparation method thereof. The thermal barrier coating is sequentially composed of a first bonding layer, a second bonding layer, a ceramic transition layer and a ceramic layer from bottom to top. The first bonding layer or the second bonding layer is made of one or more of NiCoCrAlY, NiCrAlY or NiCoCrAlYTa, the thickness of the first bonding layer ranges from 70 m to 80 m, and the thickness of the second bonding layer ranges from 50 m to 70 m; the material of the ceramic transition layer or the ceramic layer is composed of RETaO4 and one of YSZ and Gd2Zr2O7, wherein RE is one or more of Y, Gd and Ho; the molar ratio of RETaO4 to YSZ or Gd2Zr2O7 is (1 to 3): 1; the thickness of the ceramic transition layer ranges from 100 m to 120 m, and the thickness of the ceramic layer ranges from 200 m to 320 m. The thermal barrier coating applied to the surface of the nickel-based alloy is obviously superior to the prior art in heat insulation performance and thermal shock resistance, and is suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic coatings, and in particular relates to a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface and a preparation method thereof. Background Art

[0002] Nickel-based alloys are a type of alloy with nickel as the main component. They are widely used in many demanding applications due to their excellent performance. Nickel-based alloys can maintain high strength in high temperature environments, have good oxidation resistance, and have excellent corrosion resistance. At the same time, nickel-based alloys have good toughness, ductility and fatigue properties, and can maintain stable mechanical properties for a long time under extreme conditions. In addition, adding different types of metal elements to nickel-based alloys and further improving the various properties of nickel-based alloys through composition regulation and organizational control can further expand their scope of application. However, with the development of aerospace, the engine intake temperature is much higher than the melting point of nickel-based alloys, and thermal barrier coating systems can be used to solve the high temperature resistance problem of nickel-based alloys. Since the engine undergoes a hot and cold alternation process during use, the thermal shock resistance of the thermal barrier coating cannot be ignored.

[0003] Thermal barrier coatings widely used in nickel-based alloys include: single-layer bonding layer and single-layer ceramic layer, single-layer bonding layer and double-layer ceramic layer, and double-layer bonding layer and double-layer ceramic layer system. However, since there is no thermal insulation effect of different gradients in the bonding layer of the single-layer bonding layer system, the thermal insulation temperature is about 200°C, and the thermal insulation capacity does not meet the requirements; and the double-layer bonding layer has a weak thermal shock resistance due to the decrease in bonding strength due to the increase in the number of layers (at 1200°C, the number of water quenching times after 10 minutes of insulation is about 100 times).

[0004] The present invention aims to provide a nickel-based alloy surface thermal barrier coating with excellent thermal insulation and thermal shock resistance. Summary of the invention

[0005] The first object of the present invention is to provide a high temperature resistant, thermal shock resistant, thermal barrier coating on the surface of a nickel-based alloy. The second object of the present invention is to provide a method for preparing the high temperature resistant, thermal shock resistant, thermal barrier coating on the surface of a nickel-based alloy.

[0006] The first object of the present invention is achieved by providing a high temperature resistant and thermal shock resistant thermal barrier coating on a nickel-based alloy surface, the thermal barrier coating being composed of a first bonding layer, a second bonding layer, a ceramic transition layer and a ceramic layer in order from bottom to top; The material of the first bonding layer or the second bonding layer is one or more of NiCoCrAlY, NiCrAlY or NiCoCrAlYTa, the thickness of the first bonding layer is 70 to 80µm, and the thickness of the second bonding layer is 50 to 70µm; the molar ratio of RETaO4 to YSZ or Gd2Zr2O7 is 1 to 3:1; The material of the ceramic transition layer or ceramic layer is composed of RETaO4 and one of YSZ and Gd2Zr2O7, wherein RE is one or more of Y, Gd and Ho; The thickness of the ceramic transition layer is 100-120 μm, and the thickness of the ceramic layer is 200-320 μm.

[0007] The maximum heat insulation temperature of the thermal barrier coating at 1500°C is 437°C; the thermal shock resistance of the thermal barrier coating is: the maximum number of water quenching times after keeping warm at 1200°C for 10 minutes is 347 times.

[0008] The second object of the present invention is achieved by the method for preparing the high temperature resistant thermal shock resistant thermal barrier coating on the surface of the nickel-based alloy, which is achieved by the following steps: 1) Sandblasting the surface of the nickel-based alloy; 2) The first and second bonding layers of the nickel-based alloy after sandblasting are sprayed in sequence by vacuum plasma spraying and supersonic flame spraying, and then left to stand in the air for 10 to 15 minutes; 3) The ceramic transition layer and the ceramic layer are sprayed in sequence by atmospheric plasma spraying and supersonic flame spraying respectively.

[0009] The beneficial effects of the present invention are as follows: the thermal barrier coating applied to the surface of the nickel-based alloy of the present invention comprises a first bonding layer, a second bonding layer, a ceramic transition layer and a ceramic layer. Among them, the first bonding layer adopts a vacuum plasma spraying method to reduce internal oxidation, and the second bonding layer adopts a supersonic flame spraying method to form a dense bonding layer. The surface reserves a suitable roughness so that the bonding layer and the ceramic layer are more tightly bonded, thereby improving the thermal shock resistance. The ceramic transition layer and the ceramic layer are combined with RETaO4 and YSZ or Gd2Zr2O7 in different proportions, so that the nickel-based alloy has good high temperature resistance and good thermal shock resistance. The thermal barrier coating applied to the surface of the nickel-based alloy provided by the present invention has significantly better thermal insulation and thermal shock resistance than the prior art, and is suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 It is an overall schematic diagram of the thermal barrier coating of the present invention; Figure 2 XRD diagram of the thermal barrier coating prepared in Example 3 of the present invention; Figure 3 This is a SEM image of the surface of the thermal barrier coating prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0011] The present invention is further described below, but the present invention is not limited in any way. Any changes made based on the present invention belong to the protection scope of the present invention.

[0012] The present invention provides a high temperature resistant and thermal shock resistant thermal barrier coating on the surface of a nickel-based alloy, wherein the thermal barrier coating is composed of a first bonding layer, a second bonding layer, a ceramic transition layer and a ceramic layer in order from bottom to top; The material of the first bonding layer or the second bonding layer is one or more of NiCoCrAlY, NiCrAlY or NiCoCrAlYTa, the thickness of the first bonding layer is 70 to 80µm, and the thickness of the second bonding layer is 50 to 70µm; The material of the ceramic transition layer or ceramic layer is composed of RETaO4 and one of YSZ and Gd2Zr2O7, wherein RE is one or more of Y, Gd, and Ho; the molar ratio of RETaO4 to YSZ or Gd2Zr2O7 is 1 to 3:1; The thickness of the ceramic transition layer is 100-120 μm, and the thickness of the ceramic layer is 200-320 μm.

[0013] The particle size of the NiCoCrAlY, NiCrAlY or NiCoCrAlYTa is 90-120 μm.

[0014] The material of the first bonding layer is NiCoCrAlY, and the material of the second bonding layer is NiCoCrAlYTa; The particle size of the YSZ, RETaO4 or Gd2Zr2O7 is 45 to 90µm.

[0015] The present invention also provides a method for preparing the high temperature resistant thermal shock resistant thermal barrier coating on the surface of the nickel-based alloy, which is achieved by the following steps: 1) Sandblasting the surface of the nickel-based alloy; 2) The first and second bonding layers of the nickel-based alloy after sandblasting are sprayed in sequence by vacuum plasma spraying and supersonic flame spraying, and then left to stand in the air for 10 to 15 minutes; 3) The ceramic transition layer and the ceramic layer are sprayed in sequence by atmospheric plasma spraying and supersonic flame spraying respectively.

[0016] In step 2), the vacuum plasma spraying process parameters are: vacuum degree is 10 -4 ~ 10 -6 atm, spray gun power is 34 ~39kW, spray gun distance is 80 ~ 100 mm, gas flow rates of argon and hydrogen are 40 ~ 50L / min and 3 ~ 7L / min respectively, powder feeding rate is 1 ~5L / min, and spray gun speed is 400 ~ 800mm / s.

[0017] In step 2), the supersonic flame spraying process parameters are: oxygen pressure of 1 ~ 2MPa, propane pressure of 0.3 ~ 0.7MPa, nitrogen pressure of 0.5 ~ 0.7MPa, oxygen flow rate of 1000 ~ 1250L / h, propane flow rate of 1100 ~ 1200L / h, nitrogen flow rate of 1000 ~ 1100L / h, spray gun distance of 120 ~ 150mm, powder feeding rate of 1 ~ 5L / min, and spray gun speed of 300 ~ 500mm / s.

[0018] In step 3), the vacuum plasma spraying process parameters are: spray gun power is 40~45kW, spray gun distance is 120~150 mm, gas flow rates of argon and hydrogen are 45~50L / min and 4~8L / min respectively, powder feeding rate is 1~5L / min, and spray gun speed is 400~800mm / s.

[0019] In step 3), the supersonic flame spraying process parameters are: oxygen pressure of 2 ~ 3MPa, propane pressure of 0.5 ~1 MPa, nitrogen pressure of 0.5 ~ 0.7MPa, oxygen flow rate of 1200 ~ 1350L / h, propane flow rate of 1200 ~ 1400L / h, nitrogen flow rate of 1000 ~ 1100L / h, spray gun distance of 150 ~ 180mm, powder feeding rate of 1 ~ 5L / min, and spray gun speed of 200 ~400mm / s.

[0020] In step 1), the material used for sandblasting is quartz sand with a particle size of 1 to 2 mm and a pressure of 3 to 6 bar.

[0021] Example 1 1) Use quartz sand with a particle size of 1 mm to sandblast the surface of the nickel-based alloy at a pressure of 3 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -4atm, spray gun power is 34kW, spray gun distance is 80mm, argon and hydrogen gas flow rates are 40L / min and 3L / min respectively, powder feeding rate is 1L / min, and spray gun speed is 400mm / s; the first bonding layer material is NiCoCrAlY, with a particle size of 90µm and a thickness of 70µm. The second bonding layer is sprayed by supersonic flame spraying. The parameters are: oxygen pressure 1MPa, propane pressure 0.3MPa, nitrogen pressure 0.5MPa, oxygen flow rate 1000L∕h, propane flow rate 1100L∕h, nitrogen flow rate 1000L∕h, spray gun distance 120mm, powder feeding rate 1L / min, spray gun speed 300mm / s; the second bonding layer material is NiCrAlY, with a particle size of 120µm and a thickness of 70µm.

[0022] 3) Let the adhesive layer sprayed in step 2) stand in the air for 10 minutes; 4) Use atmospheric plasma to spray the ceramic transition layer on the coating after standing in step 3). The parameters are: spray gun power is 40kW, spray gun distance is 120mm, argon and hydrogen gas flow rates are 45L / min and 4L / min respectively, powder feeding rate is 1L / min, spray gun speed is 400mm / s; the material is a mixture of YSZ and YTaO4 in a molar ratio of 1:1, with a particle size of 45µm and a thickness of 100µm. Use supersonic flame spraying to spray the ceramic layer, and the process parameters are: oxygen pressure 2MPa, propane pressure 0.5MPa, nitrogen pressure 0.5MPa, oxygen flow rate 1200L∕h, propane flow rate 1200L∕h, nitrogen flow rate 1000L∕h, spray gun distance 150mm, powder feeding rate 1 / min, spray gun speed 200mm / s, material is Y 0.5 G 0.5 TaO4 and Gd2Zr2O7 are mixed in a molar ratio of 1:1, with a particle size of 90µm and a thickness of 320µm.

[0023] Example 2 1) Use quartz sand with a particle size of 2 mm to sandblast the surface of the nickel-based alloy at a pressure of 6 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -6atm, spray gun power is 39kW, spray gun distance is 100mm, argon and hydrogen gas flow rates are 50L / min and 7L / min respectively, powder feeding rate is 5L / min, spray gun speed is 800mm / s; the first bonding layer material is NiCrAlY, with a particle size of 120µm and a thickness of 80µm. The second bonding layer is sprayed by supersonic flame spraying. The parameters are: oxygen pressure 2MPa, propane pressure 0.7MPa, nitrogen pressure 0.7MPa, oxygen flow rate 1250L∕h, propane flow rate 1200L∕h, nitrogen flow rate 1100L∕h, spray gun distance 150mm, powder feeding rate 5L / min, spray gun speed 500mm / s; the second bonding layer material is NiCoCrAlY, with a particle size of 90µm and a thickness of 50µm.

[0024] 3) Let the adhesive layer sprayed in step 2) stand in the air for 15 minutes; 4) Use atmospheric plasma to spray the ceramic transition layer on the coating after standing in step 3). The parameters are: spray gun power is 45kW, spray gun distance is 150mm, argon and hydrogen gas flow rates are 50L / min and 8L / min respectively, powder feeding rate is 5L / min, spray gun speed is 800mm / s; the material is a mixture of YSZ and HoTaO4 in a molar ratio of 1:1, with a particle size of 90µm and a thickness of 120µm. Use supersonic flame spraying to spray the ceramic layer, and the process parameters are: oxygen pressure 3MPa, propane pressure 1MPa, nitrogen pressure 0.7MPa, oxygen flow rate 1350L∕h, propane flow rate 1400L∕h, nitrogen flow rate 1100L∕h, spray gun distance 180mm, powder feeding rate 5 / min, spray gun speed 400mm / s. The material is Y 0.5 Ho 0.5 TaO4 and Gd2Zr2O7 are mixed in a molar ratio of 2:1, with a particle size of 45µm and a thickness of 200µm.

[0025] Example 3 1) Use quartz sand with a particle size of 2 mm to sandblast the surface of the nickel-based alloy at a pressure of 4 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -5atm, spray gun power is 37kW, spray gun distance is 90mm, argon and hydrogen gas flow rates are 45L / min and 5L / min respectively, powder feeding rate is 3L / min, and spray gun speed is 600mm / s; the first bonding layer material is NiCoCrAlY, with a particle size of 100µm and a thickness of 75µm. Supersonic flame spraying is used for the second bonding layer spraying. The parameters are: oxygen pressure 2MPa, propane pressure 0.5MPa, nitrogen pressure 0.6MPa, oxygen flow rate 1150L∕h, propane flow rate 1150L∕h, nitrogen flow rate 1050L∕h, spray gun distance 130mm, powder feeding rate 3L / min, spray gun speed 400mm / s; the second bonding layer material is NiCoCrAlYTa, with a particle size of 110µm and a thickness of 60µm.

[0026] 3) Let the adhesive layer sprayed in step 2) stand in the air for 12 minutes; 4) Use atmospheric plasma to spray the ceramic transition layer on the coating after standing in step 3). The parameters are: the spray gun power is 42kW, the spray gun distance is 130mm, the gas flow rates of argon and hydrogen are 47L / min and 8L / min respectively, the powder feeding rate is 3L / min, and the spray gun speed is 600mm / s; the material is a mixture of Gd2Zr2O7 and YTaO4 in a molar ratio of 1:1, with a particle size of 60µm and a thickness of 110µm. Use supersonic flame spraying to spray the ceramic layer, and the process parameters are: oxygen pressure 3MPa, propane pressure 0.8MPa, nitrogen pressure 0.6MPa, oxygen flow rate 1300L∕h, propane flow rate 1300L∕h, nitrogen flow rate 1100L∕h, spray gun distance 160mm, powder feeding rate 3 / min, and spray gun speed 300mm / s. The material is Y 0.5 G 0.5 TaO4 and YSZ are mixed in a molar ratio of 3:1, with a particle size of 80µm and a thickness of 250µm.

[0027] Example 4 1) Use quartz sand with a particle size of 1 mm to sandblast the surface of the nickel-based alloy at a pressure of 5 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -5atm, spray gun power is 36kW, spray gun distance is 100mm, argon and hydrogen gas flow rates are 47L / min and 4L / min respectively, powder feeding rate is 4L / min, spray gun speed is 500mm / s; the first bonding layer material is NiCoCrAlYTa, with a particle size of 110µm and a thickness of 70µm. The second bonding layer is sprayed by supersonic flame spraying. The parameters are: oxygen pressure 1MPa, propane pressure 0.4MPa, nitrogen pressure 0.7MPa, oxygen flow rate 1100L∕h, propane flow rate 1100L∕h, nitrogen flow rate 1100L∕h, spray gun distance 140mm, powder feeding rate 4L / min, spray gun speed 300mm / s; the second bonding layer material is NiCoCrAlY, with a particle size of 100µm and a thickness of 50µm.

[0028] 3) Let the adhesive layer sprayed in step 2) stand in the air for 11 minutes; 4) The coating after standing in step 3) is sprayed with a ceramic transition layer using atmospheric plasma. The parameters are: the spray gun power is 44kW, the spray gun distance is 130mm, the gas flow rates of argon and hydrogen are 46L / min and 6L / min respectively, the powder feeding rate is 4L / min, and the spray gun speed is 600mm / s; the material is a mixture of Gd2Zr2O7 and HoTaO4 in a molar ratio of 1:1, with a particle size of 60µm and a thickness of 110µm. The ceramic layer is sprayed using supersonic flame spraying, and the process parameters are: oxygen pressure 3MPa, propane pressure 0.8MPa, nitrogen pressure 0.6MPa, oxygen flow rate 1300L∕h, propane flow rate 1300L∕h, nitrogen flow rate 1100L∕h, spray gun distance 160mm, powder feeding rate 3 / min, and spray gun speed 300mm / s. The material is Y 0.5 Ho 0.5 TaO4 and YSZ are mixed in a molar ratio of 2:1, with a particle size of 80µm and a thickness of 250µm.

[0029] Example 5 1) Use quartz sand with a particle size of 2 mm to sandblast the surface of the nickel-based alloy at a pressure of 6 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -6atm, spray gun power is 38kW, spray gun distance is 100mm, argon and hydrogen gas flow rates are 48L / min and 6L / min respectively, powder feeding rate is 5L / min, and spray gun speed is 700mm / s; the first bonding layer material is NiCoCrAlYTa, with a particle size of 110µm and a thickness of 70µm. The second bonding layer is sprayed by supersonic flame spraying. The parameters are: oxygen pressure 1MPa, propane pressure 0.4MPa, nitrogen pressure 0.7MPa, oxygen flow rate 1100L∕h, propane flow rate 1100L∕h, nitrogen flow rate 1100L∕h, spray gun distance 140mm, powder feeding rate 2L / min, spray gun speed 300mm / s; the second bonding layer material is NiCrAlY, with a particle size of 100µm and a thickness of 50µm.

[0030] 3) Let the adhesive layer sprayed in step 2) stand in the air for 13 minutes; 4) The coating after standing in step 3) is sprayed with a ceramic transition layer using atmospheric plasma. The parameters are: spray gun power is 42kW, spray gun distance is 140mm, argon and hydrogen gas flow rates are 48L / min and 7L / min respectively, powder feeding rate is 2L / min, spray gun speed is 600mm / s; material is Y 0.5 Ho 0.5 TaO4 and YSZ are mixed in a molar ratio of 1:1, with a particle size of 80µm and a thickness of 100µm. The ceramic layer is sprayed using supersonic flame spraying, where the process parameters are: oxygen pressure 3MPa, propane pressure 0.8MPa, nitrogen pressure 0.6MPa, oxygen flow rate 1300L / h, propane flow rate 1300L / h, nitrogen flow rate 1100L / h, spray gun distance 160mm, powder feeding rate 3 / min, and spray gun speed 300mm / s. The material is a mixture of Gd2Zr2O7 and HoTaO4 in a molar ratio of 1:1, with a particle size of 60µm and a thickness of 280µm.

[0031] Example 6 1) Use quartz sand with a particle size of 2 mm to sandblast the surface of the nickel-based alloy at a pressure of 6 bar; 2) The nickel-based alloy after sandblasting in step 1) is sprayed with the first bonding layer by vacuum plasma spraying. The parameters are: vacuum degree is 10 -6atm, spray gun power is 39kW, spray gun distance is 100mm, argon and hydrogen gas flow rates are 49L / min and 4L / min respectively, powder feeding rate is 2L / min, spray gun speed is 500mm / s; the first bonding layer material is NiCrAlY, with a particle size of 90µm and a thickness of 80µm. The second bonding layer is sprayed by supersonic flame spraying. The parameters are: oxygen pressure 1MPa, propane pressure 0.4MPa, nitrogen pressure 0.7MPa, oxygen flow rate 1100L∕h, propane flow rate 1100L∕h, nitrogen flow rate 1100L∕h, spray gun distance 150mm, powder feeding rate 2L / min, spray gun speed 400mm / s; the second bonding layer material is NiCoCrAlYTa, with a particle size of 100µm and a thickness of 70µm.

[0032] 3) Let the adhesive layer sprayed in step 2) stand in the air for 12 minutes; 4) The coating after standing in step 3) is sprayed with a ceramic transition layer using atmospheric plasma. The parameters are: spray gun power is 41kW, spray gun distance is 110mm, argon and hydrogen gas flow rates are 49L / min and 5L / min respectively, powder feeding rate is 3L / min, spray gun speed is 800mm / s; material is Y 0.5 Ho 0.5 TaO4 and Gd2Zr2O7 are mixed in a molar ratio of 1:1, with a particle size of 80µm and a thickness of 100µm. The ceramic layer is sprayed using supersonic flame spraying, where the process parameters are: oxygen pressure 3MPa, propane pressure 0.8MPa, nitrogen pressure 0.6MPa, oxygen flow 1300L / h, propane flow 1300L / h, nitrogen flow 1100L / h, spray gun distance 180mm, powder feeding rate 2 / min, spray gun speed 400mm / s. The material is Y 0.5 G 0.5 TaO4 and YSZ are mixed in a molar ratio of 1:1, with a particle size of 60µm and a thickness of 280µm.

[0033] Comparative Example 1 The difference from Example 1 is that both the first bonding layer and the second bonding layer are sprayed by vacuum plasma.

[0034] Comparative Example 2 The difference from Example 1 is that both the first bonding layer and the second bonding layer are sprayed by supersonic flame.

[0035] Comparative Example 3 The difference from Example 1 is that both the first bonding layer and the second bonding layer are sprayed by atmospheric plasma.

[0036] Comparative Example 4 The difference from Example 1 is that the ceramic transition layer material is YTaO4 and the ceramic layer material is Gd2Zr2O7.

[0037] Comparative Example 5 The difference from Example 1 is that the ceramic transition layer material is YSZ and the ceramic layer material is Y 0.5 G 0.5 TaO4.

[0038] Comparative Example 6 The difference from Example 1 is that Y 0.5 G 0.5 TaO4 and Gd2Zr2O7 are mixed in a molar ratio of 4:1.

[0039] Comparative Example 7 The difference from Example 1 is that vacuum plasma sprayed metal Ta is used as the first bonding layer, Ta2O5 is used as the second bonding layer, atmospheric plasma sprayed YTaO4 is used as the ceramic layer transition layer, and Y3TaO7 is used as the ceramic layer.

[0040] Experimental example 1. XRD characterization: The coatings obtained in Examples 1 to 6 and Comparative Examples 1 to 7 were tested using an X-ray diffractometer. Taking the coating obtained in Example 3 as an example, its XRD pattern is as follows: Figure 2 As shown, the XRD test results of Example 3 show that t-phase RETaO4 is mixed with t-phase ZrO2 without segregation.

[0041] 2. SEM characterization: The surfaces of the coatings obtained in Examples 1 to 6 and Comparative Examples 1 to 7 were detected using a scanning electron microscope. Taking the coating obtained in Example 3 as an example, its SEM spectrum is as follows: Figure 3 As shown, according to Figure 3 It is observed that the powder material melts evenly and there are some microcracks on the surface. These microcracks can relieve the thermal stress caused by thermal expansion and improve the thermal shock resistance.

[0042] 3. Determination of thermal insulation cooling gradient After preparing the coatings of Examples 1 to 6 and Comparative Examples 1 to 7 on the surface of a nickel-based alloy disc with a diameter of 25.4 mm, the thermal insulation cooling gradient was tested. The coating surface was heated to 1500°C within 20 seconds by an acetylene + oxygen spray gun, and the coating surface temperature (T1=1500°C) was tested using an infrared tester. The temperature was kept at 1500°C for 30 seconds, and the back temperature (T2) of the nickel-based alloy was tested using a thermocouple. The difference between T1 and T2 is the thermal insulation cooling gradient of the coating (ΔT=T1-T2). Each sample coating was tested 20 times and the average value was taken.

[0043] Results: As shown in Table 1, the thermal insulation and cooling gradients of the thermal barrier coatings prepared in Examples 1 to 6 are significantly higher than those in Comparative Examples 1 to 7.

[0044] Table 1 Thermal insulation cooling gradient of Examples 1 to 6 and Comparative Examples 1 to 7

[0045] 4. Thermal shock performance measurement After the coatings of Examples 1 to 6 and Comparative Examples 1 to 7 were prepared on the surface of a nickel-based alloy disc with a diameter of 25.4 mm, the thermal shock resistance thereof was tested. The sample was placed in a 1200°C tubular furnace for 10 minutes, taken out and placed in normal temperature water for cooling, and then placed in the tubular furnace again for one cycle. When the surface coating peeling area exceeds 10% of the total area, the coating is considered to have failed.

[0046] Results: As shown in Table 2, the number of thermal shock cycles of Examples 1 to 6 is significantly better than that of Comparative Examples 1 to 7, wherein the number of thermal shock cycles of Example 3 is as high as 374 times.

[0047] Table 2 Number of thermal shock cycles of Examples 1 to 6 and Comparative Examples 1 to 7 The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface, characterized in that: It is composed of a first bonding layer, a second bonding layer, a ceramic transition layer and a ceramic layer from bottom to top; The material of the first bonding layer or the second bonding layer is one or more of NiCoCrAlY, NiCrAlY or NiCoCrAlYTa, the thickness of the first bonding layer is 70 to 80µm, and the thickness of the second bonding layer is 50 to 70µm; The material of the ceramic transition layer or ceramic layer is composed of RETaO4 and one of YSZ and Gd2Zr2O7, wherein RE is one or more of Y, Gd, and Ho; the molar ratio of RETaO4 to YSZ or Gd2Zr2O7 is 1 to 3:1; The thickness of the ceramic transition layer is 100-120 μm, and the thickness of the ceramic layer is 200-320 μm.

2. The high temperature resistant, thermal shock resistant, thermal barrier coating on the surface of the nickel-based alloy according to claim 1, characterized in that: The maximum heat insulation temperature of the thermal barrier coating at 1500°C is 437°C; the thermal shock resistance of the thermal barrier coating is: the maximum number of water quenching times after keeping warm at 1200°C for 10 minutes is 347 times.

3. The high temperature resistant, thermal shock resistant, thermal barrier coating on the surface of nickel-based alloy according to claim 1, characterized in that: The particle size of the NiCoCrAlY, NiCrAlY or NiCoCrAlYTa is 90 to 120 μm; the particle size of the YSZ, RETaO4 or Gd2Zr2O7 is 45 to 90 μm.

4. The high temperature resistant, thermal shock resistant and thermal barrier coating on the surface of the nickel-based alloy according to claim 1, characterized in that: The material of the first bonding layer is NiCoCrAlY, and the material of the second bonding layer is NiCoCrAlYTa.

5. The method for preparing the high temperature resistant, thermal shock resistant and thermal barrier coating on the surface of the nickel-based alloy according to claim 1, characterized in that: To do this, follow these steps: 1) Sandblasting the surface of the nickel-based alloy; 2) The first and second bonding layers of the nickel-based alloy after sandblasting are sprayed in sequence by vacuum plasma spraying and supersonic flame spraying, and then left to stand in the air for 10 to 15 minutes; 3) The ceramic transition layer and the ceramic layer are sprayed in sequence by atmospheric plasma spraying and supersonic flame spraying respectively.

6. The method for preparing a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface according to claim 5, characterized in that: In step 2), the vacuum plasma spraying process parameters are: vacuum degree is 10 -4 ~ 10 -6 atm, spray gun power is 34 ~ 39kW, spray gun distance is 80 ~ 100 mm, gas flow rates of argon and hydrogen are 40 ~ 50L / min and 3 ~ 7L / min respectively, powder feeding rate is 1 ~ 5L / min, and spray gun speed is 400 ~ 800mm / s.

7. The method for preparing a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface according to claim 5, characterized in that: In step 2), the supersonic flame spraying process parameters are: oxygen pressure of 1 ~ 2MPa, propane pressure of 0.3 ~ 0.7MPa, nitrogen pressure of 0.5 ~ 0.7MPa, oxygen flow rate of 1000 ~ 1250L∕h, propane flow rate of 1100 ~ 1200L∕h, nitrogen flow rate of 1000 ~ 1100L∕h, spray gun distance of 120 ~ 150mm, powder feeding rate of 1 ~ 5L / min, and spray gun speed of 300 ~ 500mm / s.

8. The method for preparing a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface according to claim 5, characterized in that: In step 3), the vacuum plasma spraying process parameters are: spray gun power is 40 ~ 45kW, spray gun distance is 120 ~ 150 mm, gas flow rates of argon and hydrogen are 45 ~ 50L / min and 4 ~ 8L / min respectively, powder feeding rate is 1 ~ 5L / min, and spray gun speed is 400 ~ 800mm / s.

9. The method for preparing a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface according to claim 5, characterized in that: In step 3), the supersonic flame spraying process parameters are: oxygen pressure of 2 ~ 3MPa, propane pressure of 0.5 ~ 1MPa, nitrogen pressure of 0.5 ~ 0.7MPa, oxygen flow rate of 1200 ~ 1350L∕h, propane flow rate of 1200 ~ 1400L∕h, nitrogen flow rate of 1000 ~ 1100L∕h, spray gun distance of 150 ~ 180mm, powder feeding rate of 1 ~ 5L / min, and spray gun speed of 200 ~400mm / s.

10. The method for preparing a high temperature resistant, thermal shock resistant, thermal barrier coating on a nickel-based alloy surface according to claim 5, characterized in that: In step 1), the material used for sandblasting is quartz sand with a particle size of 1 to 2 mm and a pressure of 3 to 6 bar.

Citation Information

Patent Citations

  • Preparation method of thermal barrier coating containing bilayer structure of bonding layers

    CN104674217A

  • Target and its production and formation of film high in refractive index

    JP1996158048A

  • Thermal barrier coating system, components coated therewith and method for applying a thermal barrier coating system to components

    US20110300357A1

  • Novel architectures for ultra low thermal conductivity thermal barrier coatings with improved erosion and impact properties

    US20150233256A1

Cited By

  • Preparation method of nickel-based superalloy K435 thermal barrier coating

    CN119800273A

  • A method for preparing a thermal barrier coating of nickel-based superalloy K435

    CN119800273B